Coated precursor of positive electrode material, coated positive electrode material, preparation method and application
By using LiAlCl2O to coat the precursor to form LiCl, LiAlCl4 and Al2O3 coating layers under low temperature conditions, the interface problem of high nickel ternary positive electrode and sulfide electrolyte is solved, the stability and performance of the battery are improved, and the high energy density is met and high power density requirements.
Patent Information
- Application Number
- CN202411001967.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
When the prior art solves the interface problem between the high-nickel ternary positive electrode and the sulfide electrolyte, the cladding layer lacks ionic conductivity and uniformity, and the high-temperature cladding method may lead to the damage of the positive electrode structure and affect the battery performance.
LiAlCl2O is used as the coating precursor, and through low-temperature melt heating and specific charging methods, the LiCl, LiAlCl4 and Al2O3 coating layers are decomposed in situ during the first week of the battery to form a uniform surface coating and ionic conductivity.
It improves the stability, life and rate performance of the battery, avoids the damage to the positive electrode structure, and meets the needs of high energy density, safety and high power density.
Smart Images

Figure HDA0004961852800000011 
Figure HDA0004961852800000012 
Figure HDA0004961852800000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries, and in particular relates to a coated precursor of a positive electrode material, a coated positive electrode material, and a preparation method and application thereof. Background Art
[0002] As the global demand for new energy sources grows, batteries are increasingly used as efficient and clean energy storage and conversion devices. Among them, all-solid-state batteries are regarded as an important development direction for the next generation of batteries due to their advantages such as high energy density, high safety and long cycle life. However, one of the key technical challenges of all-solid-state batteries is how to solve the interface problem between the high-nickel ternary positive electrode and the sulfide electrolyte. This is because the high-nickel ternary positive electrode has extremely high reactivity, which will lead to the decomposition and degradation of the sulfide electrolyte, thus affecting the performance of the battery.
[0003] In order to solve this problem, the prior art usually adopts a method of coating the surface of the ternary positive electrode to reduce the interfacial reaction between the active material and the electrolyte. This method usually uses inert materials such as aluminum oxide or titanium dioxide for coating. However, this method has some problems. For example, the oxide used in the coating layer does not have ion conductivity, which will affect the ion transfer between the positive electrode active material and the electrolyte, thereby affecting the battery's rate performance and capacity. In addition, the uniformity of the coating layer is also a problem, because even if nano-scale aluminum oxide and titanium oxide particles are used, they will inevitably agglomerate during the coating process, forming a point coating instead of a uniform surface coating.
[0004] In summary, there are several major problems with the existing ternary positive electrode surface coating methods. First, the oxide used in the coating layer does not have ion conductivity, which will affect the ion transfer between the positive electrode active material and the electrolyte, thereby affecting the battery's rate performance and capacity. Secondly, the uniformity of the coating layer is a problem, because even if nano-scale aluminum oxide and titanium oxide particles are used, they will inevitably agglomerate during the coating process, forming a point coating rather than a uniform surface coating. Finally, the existing coating methods are usually carried out at high temperatures, which may cause structural damage to the ternary positive electrode, thereby affecting the performance of the battery.
[0005] Therefore, it is a problem to be solved to provide a ternary positive electrode material that can be prepared under low temperature conditions, has a uniform coating and has an ion conductive coating layer. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a coated precursor of a positive electrode material, a coated positive electrode material, a preparation method and an application. The coating layer of the coated positive electrode material provided by the present invention can be prepared under lower temperature conditions, and the coating layer is uniformly coated and has ion conductivity.
[0007] The invention provides a coating precursor of a positive electrode material, wherein the coating precursor is LiAlCl2O.
[0008] Preferably, the method for preparing the coated precursor comprises the following steps:
[0009] LiCl, AlCl3 and Al2O3 are mixed and heated to react under protective atmosphere to obtain LiAlCl2O.
[0010] Preferably, the protective atmosphere condition is argon, nitrogen or vacuum atmosphere.
[0011] Preferably, the temperature of the heating reaction is 450-550°C.
[0012] The present invention also provides a coated positive electrode material, comprising a positive electrode active substance and a coating layer coated on the surface of the positive electrode active substance, wherein the coating layer is prepared from the above-mentioned coating precursor.
[0013] Preferably, the coating layer comprises LiCl, AlCl3 and Al2O3.
[0014] The present invention also provides a method for preparing the above-mentioned coated positive electrode material, comprising the following steps:
[0015] Mixing a coated precursor with a positive electrode active material to obtain a mixture, and heating the mixture under protective atmosphere conditions to obtain a positive electrode material coated with the precursor;
[0016] The positive electrode material coated with the precursor is charged to obtain a coated positive electrode material.
[0017] Preferably, the coating precursor accounts for 0.1 wt% to 5 wt% of the mixture;
[0018] The protective atmosphere condition is argon, nitrogen or vacuum atmosphere, the heating temperature is 150-200° C., and the heating time is 30-180 min.
[0019] Preferably, the charging conditions are:
[0020] Set the charging rate to 0.01C ~ 0.05C; when the positive electrode potential rises to between 3.5 and 3.8V, let it stand at this potential for 60 to 180 minutes; then, continue charging to 3.8 to 3.9V, and let it stand at this potential for 30 to 180 minutes.
[0021] The present invention also provides an all-solid-state battery, comprising the above-mentioned coated positive electrode material.
[0022] Compared with the prior art, the present invention provides a coating precursor of a positive electrode material, wherein the coating precursor is LiAlCl2O. The present invention uses LiAlCl2O as a precursor of the coating layer to prepare a coated positive electrode material, obtains a positive electrode material coated with LiAlCl2O by simple melting and heating, and then, through a specific charging method, the precursor is in situ decomposed to produce LiCl, LiAlCl4 and Al2O3 to form a coating layer, and the formed coating layer is more uniform and has ion conductivity. The coating layer provided by the present invention has the characteristics of uniform surface coating, and compared with the point coating in the prior art, it can more effectively isolate the direct contact between the positive electrode active material and the electrolyte, thereby reducing the interfacial reaction and improving the stability and life of the battery. The coating layer of the present invention is composed of an oxidation-resistant substance and an ion-conductive substance uniformly mixed at the molecular level, which can not only isolate the direct contact between the positive electrode active material and the electrolyte, but also construct an ion channel in the coating layer, so that the influence of the coating layer on the battery rate is minimized. The coating layer in the present invention is formed in situ during the charging process. Compared with the high-temperature coating method in the prior art, the coating process of the present invention is more gentle and will not cause structural damage to the ternary positive electrode, thereby ensuring the performance of the battery. The coating agent precursor of the present invention has the characteristic of decomposing at a voltage above 3.5V. This characteristic enables the coating agent precursor to decompose during the first week of battery charging to form a coating product. It is a new coating method. The three coatings obtained have the characteristics of molecular-level mixing, are evenly distributed on the surface of the positive electrode particles, and present a uniform surface coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a photograph of the precursor in a molten state;
[0024] Figure 2 is the SEM image of the precursor powder;
[0025] Figure 3 is the XRD pattern of the precursor powder;
[0026] Figure 4 This is a photo of the mixed material of the precursor and the positive electrode active material;
[0027] Figure 5 This is the SEM image of the mixed material of the precursor and the positive electrode active material;
[0028] Figure 6 is the SEM image of the positive electrode active material before heating;
[0029] Figure 7 This is the SEM image of the precursor coated with the positive electrode active material after heating;
[0030] Figure 8 is the test result of the decomposition potential of the precursor;
[0031] Fig. 9 This is the EDS characterization result of the coated positive electrode active material;
[0032] Fig.10 The first week charge and discharge curve of the battery prepared in Example 1;
[0033] Fig.11 The rate performance test results of the battery prepared in Example 1. DETAILED DESCRIPTION
[0034] The present invention provides a coating precursor of a positive electrode material, wherein the coating precursor is LiAlCl2O. LiAlCl2O is a substance having the property of melting at low temperature, and the melting point of LiAlCl2O is 170±20° C. The phase state of the coating precursor is a glass-ceramic mixed phase.
[0035] The method for preparing the coated precursor comprises the following steps:
[0036] LiCl, AlCl3 and Bi2O3 are mixed and heated to react under protective atmosphere to obtain LiAlCl2O, wherein the molar ratio of LiCl, AlCl3 and Bi2O3 is 3:3:1.
[0037] Among them, the reaction formula is as follows:
[0038] 3LiCl+3AlCl3+Bi2O3=3LiAlCl2O+2BiCl3;
[0039] The present invention utilizes the boiling point of BiCl3 of 447°C, heats the reaction to above 450°C under vacuum, discharges BiCl3 gas, and obtains LiAlCl2O, which is the coating precursor.
[0040] The protective atmosphere condition is an inert atmosphere, nitrogen or vacuum atmosphere. The inert atmosphere can be argon. The protective atmosphere condition is preferably a vacuum atmosphere.
[0041] The temperature of the heating reaction is 450-550°C, and can be 450, 455, 460, 470, 480, 490, 500, 510, 520, 530, 540, 550, or any value between 450 and 550°C.
[0042] In order to better obtain contact with the positive electrode active material in the next step, the prepared precursor is crushed into powder for standby use. The present invention has no particular limitation on the crushing method, and any crushing method known to those skilled in the art can be used. In the present invention, the crushing method can be grinding, ball milling or high-speed mixing.
[0043] The present invention also provides a coated positive electrode material, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material, wherein the coating layer is prepared from the above-mentioned coating precursor. Specifically, the coating layer is obtained by heating and melting the coating precursor and then charging it.
[0044] Wherein, the coating layer comprises LiCl, LiAlCl4 and Al2O3, and the molar ratio of LiCl, LiAlCl4 and Al2O3 is 2:1:1.
[0045] Specifically, the method for preparing the coated positive electrode material comprises the following steps:
[0046] Mixing a coated precursor with a positive electrode active material to obtain a mixture, and heating the mixture under a protective atmosphere to obtain a positive electrode material coated with the precursor;
[0047] The positive electrode material coated with the precursor is charged to obtain a coated positive electrode material.
[0048] The present invention first mixes the coating precursor with the positive electrode active material to obtain a mixture. The present invention does not have any special restrictions on the mixing method, and any mixing method known to those skilled in the art can be used. Preferably, the mixing can be grinding, ball milling or high-speed mixing. The coating precursor accounts for 0.1wt% to 5wt% of the mixture, which can be 0.1wt%, 0.3wt%, 0.5wt%, 0.9wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, or any value between 0.1wt% and 5wt%. The positive electrode active material is selected from one or more of lithium nickel cobalt manganese oxide, lithium cobalt oxide, lithium nickel manganese oxide, and lithium-rich manganese-based materials.
[0049] Then, the mixture is heated under protective atmosphere conditions. The protective atmosphere conditions are argon, nitrogen or vacuum atmosphere. After the precursor is mixed with the positive electrode active material, in order to avoid degradation of the positive electrode active material at high temperature, the heating temperature is between 350 and 450°C, and can be 350, 360, 370, 380, 390, 400, 410, 420, 430, 440, 450, or any value between 350 and 450°C. The heating time is 30 to 180 minutes, and can be 30, 60, 90, 120, 150, 180, or any value between 30 and 180 minutes.
[0050] The melting point of the obtained LiAlCl2O is 170±20°C. Therefore, LiAlCl2O is mixed with the positive electrode active material and heated to above its melting point. The LiAlCl2O-coated positive electrode material can be obtained by simple melting heating.
[0051] After obtaining the positive electrode material coated with the precursor, in order to make the coating agent precursor fully and evenly decompose into the intended coating layer, the charging system needs to be set during the charging process. It is to avoid that the positive electrode potential rises to the decomposition voltage of the sulfide electrolyte before the coating layer material is fully formed, causing the decomposition of the solid electrolyte.
[0052] Specifically, during the first week of charging, the charging rate is preferably between 0.01C and 0.05C, and can be 0.01, 0.02, 0.03, 0.04, 0.05, or any value between 0.01C and 0.05C. When the positive electrode potential rises to between 3.5 and 3.8V, it can be 3.5, 3.6, 3.7, 3.8, or any value between 3.5 and 3.8V, and stand at this potential for 60 to 180 minutes, which can be 60, 90, 120, 150, 180, or any value between 60 and 180 minutes. After standing, continue to charge to 3.8 to 3.9V, and continue to stand for 30 to 180 minutes, which can be 30, 60, 90, 120, 150, 180, or any value between 30 and 180 minutes. Then the coating agent precursor completes decomposition to form a coating layer. After this, the battery can go through normal charge and discharge cycles.
[0053] In the present invention, the coating agent precursor has the characteristic of decomposing above a voltage of 3.5V (vs Li). When the voltage is increased to the decomposition voltage, the coating agent precursor undergoes the following decomposition reaction: 3LiAlCl2O=2LiCl+LiAlCl4+Al2O3, so that the coating agent precursor can be decomposed during the first week of charging of the battery to form a coated product. Among them, LiCl and Al2O3 have the characteristics of high pressure resistance, and LiAlCl4 has ionic conductivity; therefore, LiCl and Al2O3 play a role in physically blocking the contact between the positive electrode active material and the electrolyte, and LiAlCl4 constructs an ion channel therein. Since the above-mentioned coating is produced by the in-situ decomposition of the coating precursor, the three coatings have the characteristics of molecular-level mixing, are evenly distributed on the surface of the positive electrode particles, and present a uniform surface coating.
[0054] The present invention also provides an all-solid-state battery, comprising the above-mentioned coated positive electrode material.
[0055] In the present invention, the all-solid-state battery comprises a positive electrode, a negative electrode and a solid electrolyte, wherein the positive electrode comprises a positive electrode active material, and the positive electrode active material is selected from the above-mentioned coated positive electrode material.
[0056] The negative electrode is selected from one or more of lithium metal, lithium alloy, graphite, hard carbon, soft carbon, silicon oxygen, and silicon carbon.
[0057] The solid electrolyte is selected from sulfide electrolytes, preferably halide electrolytes, oxide electrolytes, and polymer electrolytes.
[0058] The present invention uses LiAlCl2O as the precursor of the coating layer to prepare a coated positive electrode material, obtains the LiAlCl2O coated positive electrode material by simple melting heating, and then, through a specific charging method, the precursor is in situ decomposed to produce LiCl, AlCl3 and Bi2O3 to form a coating layer, and the formed coating layer is more uniform and has ion conductivity. The coating layer provided by the present invention has the characteristics of uniform surface coating, which can more effectively isolate the direct contact between the positive electrode active material and the electrolyte compared to the point coating in the prior art, thereby reducing the interfacial reaction and improving the stability and life of the battery. The coating layer of the present invention is composed of an oxidation-resistant substance and an ion-conductive substance uniformly mixed at the molecular level, which can not only isolate the direct contact between the positive electrode active material and the electrolyte, but also construct an ion channel in the coating layer, so that the coating layer The influence of the battery rate is minimized. The coating layer in the present invention is formed in situ during the charging process. Compared with the high-temperature coating method in the prior art, the coating process of the present invention is more gentle and will not cause structural damage to the ternary positive electrode, thereby ensuring the performance of the battery. The coating agent precursor of the present invention has the characteristic of decomposing at a voltage above 3.5V. This characteristic enables the coating agent precursor to decompose during the first week of battery charging to form a coating product. This is a new coating method. The three coatings obtained have the characteristics of molecular-level mixing, are evenly distributed on the surface of the positive electrode particles, and present a uniform surface coating.
[0059] The in-situ coating method of the present invention can effectively solve the interface problem between the high-nickel ternary positive electrode and the sulfide electrolyte, improve the energy density, safety and cycle life of the battery, and meet the market demand for high energy density and high safety batteries. At the same time, the coating layer of the present invention has the characteristics of uniform surface coating, as well as excellent ionic conductivity and oxidation resistance, which can improve the rate performance and capacity of the battery, and meet the market demand for high power density batteries. In addition, the coating method of the present invention is carried out at low temperature, which can avoid structural damage to the ternary positive electrode, improve the performance of the battery, and meet the market demand for high-performance batteries.
[0060] In order to further understand the present invention, the coated precursor of the positive electrode material, the coated positive electrode material, the preparation method and the application provided by the present invention are described below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0061] Embodiment 1:
[0062] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to the molar stoichiometry of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace and heated to 455°C under vacuum conditions. After keeping the temperature for 3 hours, the LiAlCl2O coating agent precursor was generated. At this time, the precursor was in a molten state, such as Figure 1 As shown, Figure 1 This is a photograph of the precursor in the molten state.
[0063] In order to better obtain contact with the positive electrode active material in the next step, the molten precursor is cooled and crushed into powder using a crusher. The SEM and XRD spectra of the crushed powder are as follows: Figure 2 and Figure 3 shown. Figure 2 is the SEM image of the precursor powder. Figure 3 is the XRD pattern of the precursor powder.
[0064] It can be seen from the XRD results that the phase of the precursor is a glass-ceramic mixed phase.
[0065] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, with a mixing speed of 60 rpm and a mixing time of 60 min. The photo of the mixed material is as follows Figure 4 As shown, Figure 4 The photo of the mixed material of the precursor and the positive electrode active material is shown in Figure 2. Figure 5 , Figure 5 The SEM image of the precursor and the positive electrode active material mixture. It can be seen from the SEM image that the active material NCM955 particles and the coating agent precursor particles are simply mixed together.
[0066] The mass of the coating agent precursor accounts for 4% of the above mixture.
[0067] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0068] The changes of the positive electrode active material particles before and after heating are shown in Figure 2. Figure 6 and Figure 7 As shown, Figure 6 This is the SEM image of the positive electrode active material before heating. Figure 7 This is a SEM image of the precursor coating the positive electrode active material after heating. It can be seen that after heating, the coating agent precursor is uniformly melted on the surface of the positive electrode active material, forming a uniform coating of the precursor on the positive electrode active material.
[0069] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing above a voltage of 3.5 V (vs Li). The decomposition potential is tested as follows: Figure 8 shown. Figure 8 This is the test result of the decomposition potential of the precursor.
[0070] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.8V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer. EDS was used to characterize the element distribution of the positive electrode active material after the coating layer was formed, such as Fig. 9 shown. Fig. 9 This is the EDS characterization result of the coated positive electrode active material. Fig. 9 It can be seen that the target characteristic elements Cl, Al, and O are evenly distributed on the surface of the positive electrode particles and present a uniform surface coating.
[0071] Example 2
[0072] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 500°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0073] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 by a grinder, with a mixing speed of 60 rpm and a mixing time of 60 min.
[0074] The active material NCM955 particles and the coating agent precursor particles are simply mixed together.
[0075] The mass of the coating agent precursor accounts for 0.1% of the above mixture.
[0076] The mixture is then heated at 150° C. in an argon atmosphere to cause the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0077] After heating, the coating agent precursor is uniformly melted on the surface of the positive electrode active material, forming a uniform coating of the positive electrode active material by the precursor.
[0078] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0079] During the first week of charging, the charging rate was 0.01C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.5V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0080] Example 3
[0081] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to the molar stoichiometry of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 550°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0082] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min.
[0083] The active material NCM955 particles and the coating agent precursor particles are simply mixed together.
[0084] The mass of the coating agent precursor accounts for 0.5% of the above mixture.
[0085] The mixture is then heated at 200° C. in an argon atmosphere to cause the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0086] After heating, the coating agent precursor is uniformly melted on the surface of the positive electrode active material, forming a uniform coating of the positive electrode active material by the precursor.
[0087] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0088] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.9V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0089] Example 4
[0090] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 470°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0091] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 by a grinder, with a mixing speed of 60 rpm and a mixing time of 60 min.
[0092] The active material NCM955 particles and the coating agent precursor particles are simply mixed together.
[0093] The mass of the coating agent precursor accounts for 1% of the above mixture.
[0094] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0095] After heating, the coating agent precursor is uniformly melted on the surface of the positive electrode active material, forming a uniform coating of the positive electrode active material by the precursor.
[0096] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0097] During the first week of charging, the charging rate was 0.03C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.8V and left at this potential for another 90 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0098] Example 5
[0099] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 490°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0100] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 by a grinder, with a mixing speed of 60 rpm and a mixing time of 60 min.
[0101] The active material NCM955 particles and the coating agent precursor particles are simply mixed together.
[0102] The mass of the coating agent precursor accounts for 3% of the above mixture.
[0103] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0104] After heating, the coating agent precursor is uniformly melted on the surface of the positive electrode active material, forming a uniform coating of the positive electrode active material by the precursor.
[0105] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0106] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 130 minutes. After standing, it was charged to 3.9V and left at this potential for another 130 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0107] Example 6
[0108] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 530°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0109] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min.
[0110] The active material NCM955 particles and the coating agent precursor particles are simply mixed together.
[0111] The mass of the coating agent precursor accounts for 5% of the above mixture.
[0112] The mixture is then heated at 190° C. in an argon atmosphere to cause the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0113] After heating, the coating agent precursor is uniformly melted on the surface of the positive electrode active material, forming a uniform coating of the positive electrode active material by the precursor.
[0114] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0115] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 160 minutes. After standing, it was charged to 3.9V and left at this potential for 180 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0116] Comparative Example 1
[0117] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0118] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 0.05% of the above mixture.
[0119] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0120] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0121] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.8V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0122] Comparative Example 2
[0123] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0124] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 8% of the above mixture.
[0125] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0126] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0127] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.8V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0128] Comparative Example 3
[0129] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0130] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 4% of the above mixture.
[0131] The mixture was then heated at 120°C under an argon atmosphere.
[0132] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0133] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.8V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0134] Comparative Example 4
[0135] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0136] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 4% of the above mixture.
[0137] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0138] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0139] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.8V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0140] Comparative Example 5
[0141] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0142] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 4% of the above mixture.
[0143] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0144] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0145] During the first week of charging, the charging rate was 1C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 120 minutes. After standing, it was charged to 3.8V and left at this potential for another 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0146] Comparative Example 6
[0147] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0148] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 4% of the above mixture.
[0149] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0150] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0151] During the first week of charging, the charging rate was 0.05 C. When the positive electrode potential was raised to 4 V (vs Li), it was left at this potential for 120 min.
[0152] Comparative Example 7
[0153] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0154] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 4% of the above mixture.
[0155] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0156] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0157] During the first week of charging, the charging rate was 0.05 C. When the positive electrode potential rose to 3.1 V (vs Li), it was left at this potential for 120 min.
[0158] Comparative Example 8
[0159] 1. Synthesis of coating precursor: LiCl, AlCl3, and Bi2O3 were mixed in a ball mill at 400 rpm for 3 hours according to a molar stoichiometric ratio of 3:3:1 to obtain a mixture of the above substances. The mixture was then placed in a vacuum tube furnace, heated to 455°C under vacuum conditions, and kept warm for 3 hours to generate a LiAlCl2O coating agent precursor. In order to better obtain contact with the positive electrode active material in the next step, a crusher was used in this step to crush the above molten electrolyte into a powder state.
[0160] 2. Precursor coating of positive electrode active material: In this step, the precursor powder prepared in step 1 is first mixed with the positive electrode active material NCM955 through a grinder, the mixing speed is 60 rpm, and the mixing time is 60 min. The mass of the coating agent precursor accounts for 4% of the above mixture.
[0161] The mixture was then heated at 170° C. in an argon atmosphere to allow the coating precursor to melt and flow, thereby coating the surface of the positive electrode active material.
[0162] 3. Formation of coating: The coating agent precursor has the characteristic of decomposing at a voltage above 3.5 V (vs Li).
[0163] During the first week of charging, the charging rate was 0.05C. When the positive electrode potential rose to 3.6V (vs Li), it was left at this potential for 5 minutes. After standing, it was charged to 3.8V and left at this potential for 60 minutes. Then the coating agent precursor was decomposed to form a coating layer.
[0164] Comparative Example 9
[0165] NCM955 without any treatment was used as the active substance.
[0166] Comparative Example 10
[0167] Nano-alumina and positive electrode active material NCM955 were mixed with each other in a mass ratio of 1:99, and then sintered at 800°C in an oxygen atmosphere for 6 hours.
[0168] Comparative Example 11
[0169] Al2O3, LiAlCl4 and LiCl were mixed in a molar ratio of 1:1:2 to form a mixture, and then the mixture was mixed with the positive electrode active material NCM955 in a mass ratio of 1:99, and then sintered in an oxygen atmosphere at 800°C for 6 hours.
[0170] Performance Testing
[0171] Full battery test
[0172] Cycle performance and rate performance test:
[0173] (1) Preparation of positive electrode sheet:
[0174] The sulfide solid electrolyte Li6PS5Cl, the conductive agent Super P, the coated positive electrode material prepared above, and the binder PTFE were mixed in a mass ratio of 23:2:75:1 to prepare a positive electrode sheet.
[0175] (2) Assembly of all-solid-state batteries:
[0176] The sulfide solid electrolyte Li6PS5Cl was used, and the block made by pressing at 200MPa was used as the electrolyte layer. In was used as the negative electrode, and a full battery structure of positive electrode sheet / electrolyte layer / In was assembled. The rate performance and cycle performance were tested in the voltage range of 3 to 4.3V (vs Li).
[0177] The first week charge and discharge curve and rate performance test of Example 1 are as follows: Fig.10 and Fig.11 shown. Fig.10 The first week charge and discharge curve of the battery prepared in Example 1, Fig.11 The rate performance test results of the battery prepared in Example 1.
[0178] The first efficiency, rate performance and cycle performance of each embodiment and comparative example are shown in Table 1.
[0179] Table 1
[0180] Serial number First effect Magnification 1C / 0.1C 500-week cycle retention rate Example 1 90.4% 79.3% 86.1% Example 2 85.8% 85.6% 79.3% Example 3 86.1% 82.8% 80.7% Example 4 88.7% 82.1% 82.3% Example 5 89.3% 80.7% 83.6% Example 6 91.5% 77.4% 88.5% Comparative Example 1 81.6% 62.9% 57.5% Comparative Example 2 87.2% 52.5% 85.2% Comparative Example 3 82.4% 63.6% 48.5% Comparative Example 4 74.1% 43.2% 29.5% Comparative Example 5 83.2% 68.3% 74.2% Comparative Example 6 82.5% 64.6% 76.2% Comparative Example 7 82.6% 65.3% 74.7% Comparative Example 8 83.5% 66.2% 73.6% Comparative Example 9 77.3% 50.6% 31.5% Comparative Example 10 79.6 57.1 41.5% Comparative Example 11 81.6 60.5 51.3%
[0181] The coating agent content in Comparative Example 1 is too low, resulting in incomplete coating, which in turn increases the risk of contact between the electrolyte and the positive electrode active material, causing a significant decrease in cycle performance.
[0182] The coating agent content in Comparative Example 2 is too high, resulting in an overly thick coating layer, which affects the rate performance of the battery.
[0183] In comparative example 3, the coating treatment temperature was too low, so that the precursor of the coating agent could not be evenly coated on the positive electrode active material particles, forming an incomplete island coating, thereby increasing the contact risk between the electrolyte and the positive electrode active material, resulting in a significant decrease in the first efficiency and cycle performance.
[0184] In comparative example 4, the coating treatment temperature was too high, resulting in high-temperature oxygen release of the positive electrode active material, that is, the structure of the positive electrode active material collapsed, which was the main reason for the serious reduction in subsequent performance.
[0185] In comparative example 5, the charging rate was too high and the standing time was too short during the in-situ decomposition of the coating agent precursor, so that the coating agent precursor could not be completely and evenly decomposed and cracked, thereby causing a decrease in the subsequent battery performance.
[0186] In comparative example 6, the static voltage during the in-situ decomposition of the coating agent precursor was too high, so that the coating agent precursor could not be fully converted into the target coating within the main decomposition voltage range.
[0187] In the comparative example 7, the static voltage is too low during the in-situ decomposition of the coating agent precursor, and the purpose of in-situ decomposition of the coating agent precursor is not achieved.
[0188] In Comparative Example 8, the standing time during the in-situ decomposition of the coating agent precursor was too short, so that the coating agent precursor could not be fully converted into the target coating within the main decomposition voltage range.
[0189] Comparative Example 9 is a positive electrode active material without any treatment.
[0190] In comparative example 10, granular alumina was used for coating. On the one hand, it is difficult for pure alumina to form a complete surface coating, which makes it possible for the electrolyte to contact the positive electrode active material, so there is a significant difference in cycle performance compared with the example. On the other hand, alumina itself is an ion insulator, resulting in poor rate performance compared with the example.
[0191] In comparative example 11, a granular mixture is used for coating. On the one hand, it is difficult for the above mixture to form a complete planar coating on the surface of the positive electrode active material, so that there is a possibility of contact between the electrolyte and the positive electrode active material, so there is a significant difference in the cycle performance compared with the embodiment. On the other hand, the mixing between the various coating raw materials cannot achieve the molecular level mixing formed by in-situ decomposition in the embodiment, resulting in poor rate performance compared with the embodiment.
[0192] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A coated precursor of a cathode material, It is characterized in that The coating precursor is LiAlCl 2 O.
2. A method for preparing the coated precursor according to claim 1, It is characterized in that The following steps are involved: LiCl, AlCl 3 and Al 2 O 3 Mix and heat under protective atmosphere to obtain LiAlCl 2 O.
3. The preparation method according to claim 2, It is characterized in that The protective atmosphere condition is argon, nitrogen or vacuum atmosphere.
4. The preparation method according to claim 2, It is characterized in that The temperature of the heating reaction is 450-550°C.
5. A coated positive electrode material, It is characterized in that It comprises a positive electrode active material and a coating layer coated on the surface of the positive electrode active material, wherein the coating layer is prepared from the coating precursor according to claim 1.
6. The coated positive electrode material according to claim 5, It is characterized in that The coating layer includes LiCl, AlCl 3 and Al 2 O 3 .
7. A method for preparing the coated positive electrode material according to claim 5 or 6, It is characterized in that The following steps are involved: Mixing a coated precursor with a positive electrode active material to obtain a mixture, and heating the mixture under a protective atmosphere to obtain a positive electrode material coated with the precursor; The positive electrode material coated with the precursor is charged to obtain a coated positive electrode material.
8. The preparation method according to claim 7, It is characterized in that The coating precursor accounts for 0.1wt% to 5wt% of the mixture; The protective atmosphere condition is argon, nitrogen or vacuum atmosphere, the heating temperature is 150-200° C., and the heating time is 30-180 min.
9. The preparation method according to claim 7, It is characterized in that The charging conditions are: Set the charging rate to 0.01C ~ 0.05C; when the positive electrode potential rises to between 3.5 and 3.8V, let it stand at this potential for 60 to 180 minutes; then, continue charging to 3.8 to 3.9V, and let it stand at this potential for 30 to 180 minutes.
10. An all-solid-state battery, It is characterized in that Comprising the coated positive electrode material according to claim 5 or 6.