Boron-doped sodium battery positive electrode material and preparation method and application thereof

CN118929785APending Publication Date: 2024-11-12GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981400.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

[0005]因此,本发明要解决的技术问题在于克服现有包含钠电正极材料电池电学性能不佳的缺陷,从而提供一种硼掺杂钠电正极材料及其制备方法和应用

Benefits of technology

[0048] 1. The present invention provides a method for preparing a boron-doped sodium cathode material, wherein the specific steps of the preparation method include: S1, preparing Ni a Fe b Mn c (OH) 2 Precursor; S2, sodium source, boron source, Ni a Fe b Mn c (OH) 2 The precursors are mixed for the first time and sintered for the first time to obtain Na x Ni a Fe b Mn c B y O 2 One burnt product; with Ni a Fe b Mn c (OH) 2 Based on the total number of moles of metal elements in the precursor, the amount of boron element in the boron source is 0.2-5 mol%; the sodium element in the sodium source and the Ni a Fe b Mn c (OH) 2 The molar ratio of the precursor is 0.65-1.1:1; S3, the Na x Ni a Fe b Mn c B y O 2 The first fired product and coating agent are mixed for a second time and sintered for a second time to obtain a boron-doped sodium cathode material. The battery containing the boron-doped sodium cathode material prepared by the present invention has excellent charge and discharge capacity, energy density and capacity retention rate. The boron-doped sodium cathode material is a single crystal with fewer grain boundaries than polycrystalline, which reduces the occurrence of cracks during the cycle. At the same time, the single crystal produced is large in size and has a small specific surface area, which reduces the contact area between the crystal and the electrolyte. , thereby inhibiting the occurrence of some side reactions; boron element is easily incorporated into the material lattice without introducing other additional impurities. The preparation process is simple, efficient and pollution-free. The specific amount of boron source can achieve the compaction density and energy of the cathode material. dense The balance of degree; when the dosage of boron source is too high, although the compaction density is greatly increased, it will lead to a serious reduction in capacity, which is not conducive to the improvement of energy density; when the dosage of boron source is too low, although the impact on capacity is small , but at the same time, the increase in compaction density has little effect. Therefore, it is necessary to select an appropriate boron doping amount to balance the reduction in capacity after boron doping and the increase in compaction density, so that the battery that ultimately protects the cathode material has excellent capacity. Retention rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929785A_ABST
    Figure CN118929785A_ABST
Patent Text Reader

Abstract

The invention relates to the field of positive electrode materials, in particular to a boron-doped sodium battery positive electrode material and a preparation method and application thereof. The preparation method comprises the following steps: S1, preparing a NiaFebMnc (OH) 2 precursor; s2, a sodium source, a boron source and the Ni Fe Mn < c > (OH) < 2 > precursor are subjected to primary mixing and primary sintering, and a Na < x > Ni Fe Mn < c > B < y > O < 2 > primary sintering product is obtained; on the basis of the total mole number of metal elements in the NiaFebMnc (OH) 2 precursor, the dosage of the boron element in the boron source is 0.2-5 mol%; the molar ratio of the sodium element in the sodium source to the Ni Fe Mn < c > (OH) < 2 > precursor is (0.65-1.1): 1; s3, mixing the NaxNiaFebMncByO2 primary sintered product and a coating agent for the second time, and sintering for the second time to obtain the boron-doped sodium battery positive electrode material, the battery containing the prepared boron-doped sodium battery positive electrode material has excellent charge-discharge capacity, energy density and capacity retention ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a boron-doped sodium positive electrode material and a preparation method and application thereof. Background Art

[0002] With the rapid development of the new energy industry, the global demand for lithium resources has grown rapidly. However, due to the limited lithium resources in the earth's crust, it is impossible to meet the increasingly mature battery industry chain in the long term. Therefore, we have to speed up the search for a new battery material as a substitute for lithium batteries. The principle of sodium-ion batteries is similar to that of lithium-ion batteries. Both are "rocking chair batteries", but sodium is extremely abundant in the earth's energy storage, and it is low-priced and highly safe. It has received widespread attention and has been used in household energy storage, large-scale energy storage, power and other fields.

[0003] Among them, layered positive electrode materials have higher specific capacity, and the technical route is relatively mature, the production process is similar to that of lithium batteries, and the equipment is common to lithium batteries, which can achieve large-scale mass production faster. However, sodium battery polycrystalline layered transition metal oxides show poor cycle performance during long-term cycles due to cracking of polycrystalline grain boundaries and side reactions caused by contact with the electrolyte. Relatively speaking, single crystal materials can reduce contact with the electrolyte due to their smaller specific surface area, thereby inhibiting the occurrence of some side reactions. In addition, fewer grain boundaries in single crystal materials can reduce the generation of cracks during the cycle and improve electrical performance.

[0004] However, the size of the sodium-electrolyte layered oxide single crystal materials synthesized so far is relatively small, and the synthesis methods reported to increase the size of single crystals often require the addition of fluxes such as NaCl, which cannot enter the material lattice during sintering, and other impurities will be introduced during this process, which is not conducive to the material capacity and cycle stability. Therefore, it is necessary to develop a simple, efficient and pollution-free synthesis method for preparing large single crystal sodium-electrolyte positive electrode materials. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defects of poor electrical performance of existing batteries containing sodium positive electrode materials, thereby providing a boron-doped sodium positive electrode material and a preparation method and application thereof.

[0006] The first aspect of the present invention provides a method for preparing a boron-doped sodium positive electrode material, wherein the preparation method comprises the following specific steps:

[0007] S1. Preparation of Ni a Fe b Mn c (OH)2 precursor;

[0008] S2, sodium source, boron source, Ni a Fe bMn c The (OH)2 precursor is mixed for the first time and sintered for the first time to obtain Na x Ni a Fe b Mn c B y O2-burning products;

[0009] Take Ni a Fe b Mn c The amount of boron in the boron source is 0.2-5 mol%, based on the total molar amount of metal elements in the (OH)2 precursor;

[0010] The sodium element in the sodium source and Ni a Fe b Mn c The molar ratio of (OH)2 precursor is 0.65-1.1:1;

[0011] S3, the Na x Ni a Fe b Mn c B y The O2-fired product and the coating agent are mixed for the second time and sintered for the second time to obtain a boron-doped sodium positive electrode material.

[0012] In the present invention, Ni a Fe b Mn c In the (OH)2 precursor, 0.2≤a≤0.5, 0.2≤b≤0.5, 0.2≤c≤0.5, a+b+c=1; Na x Ni a Fe b Mn c B y In O2 fired products, 0.65≤x≤1.1, 0.002≤y≤0.05.

[0013] According to the present invention, Ni a Fe b Mn c The specific process of the (OH)2 precursor includes: mixing a nickel source, an iron source, a manganese source and water to obtain a mixed solution, mixing the mixed solution, a complexing agent and a pH regulator, and performing a coprecipitation reaction to obtain Ni a Fe b Mn c (OH)2 precursor.

[0014] According to the present invention, the molar ratio of the nickel element in the nickel source, the iron element in the iron source, and the manganese element in the manganese source is (0.2-0.5):(0.2-0.5):(0.2-0.5).

[0015] According to the present invention, in the mixed solution, the concentration of the metal salt solution is 3-3.5 mol / L, and the concentration of the metal salt in the metal salt solution is calculated using all the metal salts.

[0016] According to the present invention, the nickel source includes at least one of nickel sulfate, nickel chloride, nickel carbonate and nickel acetate.

[0017] According to the present invention, the iron source includes at least one of ferric sulfate, ferric chloride, ferric carbonate and ferric acetate.

[0018] According to the present invention, the manganese source includes at least one of manganese sulfate, manganese chloride, manganese carbonate and manganese acetate.

[0019] According to the present invention, the coprecipitation reaction is carried out at a temperature of 55-65° C. and for a time of 8-15 hours.

[0020] In the present invention, the coprecipitation is carried out under the protection of a protective gas such as nitrogen or an inert gas, and the flow rate of the protective gas is 6-10 L / min.

[0021] According to the present invention, when the mixed solution is added, the flow rate of the mixed solution is 5-6 L / h.

[0022] According to the present invention, in the solution where the coprecipitation reaction occurs, the pH value is 12-12.3, and the concentration of the complexing agent is 8-10 g / L.

[0023] In the present invention, the pH value refers to the pH of the entire reaction system.

[0024] In the present invention, the complexing agent and pH adjusting agent are conventional reagents in the art. Typically, but not limitedly, the complexing agent includes ammonia water and the pH adjusting agent is sodium hydroxide.

[0025] In the present invention, the complexing agent is added with water to prepare a complexing agent solution which is added into the system, and the content of the complexing agent in the complexing agent solution is 20-25wt%.

[0026] In the present invention, a pH adjuster solution prepared by adding water to a pH adjuster is added to the system to make mixing more complete. Typically, but not limiting, the content of the pH adjuster in the pH adjuster solution is 30-35 wt %.

[0027] In the present invention, after the coprecipitation reaction, the obtained product is filtered, washed and dried to obtain Ni a Fe b Mn c (OH)2 precursor.

[0028] According to the present invention, Ni a Fe b Mnc Based on the total molar amount of metal elements in the (OH)2 precursor, the amount of boron element in the boron source is 0.5-2 mol%.

[0029] According to the present invention, the sodium source includes at least one of sodium carbonate and sodium hydroxide.

[0030] According to the present invention, the boron source includes at least one of boron oxide and boric acid.

[0031] According to the present invention, the specific process of the first sintering includes: firstly heating the temperature to 500-850°C at a heating rate of 1-5°C / min and sintering for 2-6h, and then heating the temperature to 900-1200°C at a heating rate of 1-5°C / min and sintering for 5-15h.

[0032] In the present invention, the first sintering is carried out in an air atmosphere, and after the first sintering, the product is crushed and sieved to obtain Na x Ni a Fe b Mn c B y O2 burning product.

[0033] According to the present invention, the coating agent comprises at least one of a metal oxide and / or a metal salt;

[0034] According to the present invention, the metal oxide includes at least one of ZrO2, B2O3, Al2O3, CaO, TiO2, MgO, CoO, MnO, and MnO2.

[0035] According to the present invention, the metal salt includes at least one of chloride salt, bromide salt, iodide salt, nitrate salt and sulfate salt.

[0036] According to the present invention, the chloride salt includes at least one of ZrCl4, BCl3, AlCl3, CaCl2, TiCl4, MgCl2, CoCl2, and MnCl2.

[0037] According to the present invention, the bromide salt includes at least one of ZrBr4, AlBr3, CaBr2, TiBr4, MgBr2, CoBr2, and MnBr2.

[0038] According to the present invention, the iodide salt includes at least one of ZrI4, AlI3, CaI2, TiI4, MgI2, CoI2, and MnI2.

[0039] According to the present invention, the nitrate includes at least one of Zr(NO3)4, Al(NO3)3, Ca(NO3)2, Ti(NO3)2, Mg(NO3)2, Co(NO3)2, and Mn(NO3)2.

[0040] According to the present invention, the sulfate includes at least one of ZrSO4, Al2(SO4)3, MgSO4, CoSO4, and MnSO4.

[0041] According to the present invention, Na x Ni a Fe b Mn c B y Based on the mass of the O2-sintered product, the amount of the coating agent is 0.3-2wt%.

[0042] According to the present invention, the specific process of the second sintering includes: heating to 250-900° C. at a heating rate of 1-5° C. / min and sintering for 3-8 hours.

[0043] In the present invention, the second sintering is carried out in an air atmosphere, and cooling, screening and iron removal are performed after the second sintering.

[0044] In the present invention, the specific conditions for mixing, first mixing, and second mixing are conventional in the art and are not limited thereto, as long as the mixture can be mixed uniformly.

[0045] The second aspect of the present invention protects a boron-doped sodium positive electrode material prepared by the aforementioned preparation method.

[0046] A third aspect of the present invention protects a secondary battery, wherein the secondary battery comprises the aforementioned boron-doped sodium positive electrode material.

[0047] The technical solution of the present invention has the following advantages:

[0048] 1. The present invention provides a method for preparing a boron-doped sodium positive electrode material, wherein the preparation method specifically comprises the following steps: S1. preparing Ni a Fe b Mn c (OH)2 precursor; S2, sodium source, boron source, Ni a Fe b Mn c The (OH)2 precursor is mixed for the first time and sintered for the first time to obtain Na x Ni a Fe b Mn c B y O2-burning products; Ni a Fe b Mn c The total molar amount of metal elements in the (OH)2 precursor is taken as the basis, the amount of boron element in the boron source is 0.2-5 mol%; the sodium element in the sodium source and the Ni a Feb Mn c The molar ratio of (OH)2 precursor is 0.65-1.1:1; S3, the Na x Ni a Fe b Mn c B y The O2-fired product and the coating agent are mixed for the second time and sintered for the second time to obtain a boron-doped sodium positive electrode material. The battery containing the boron-doped sodium positive electrode material prepared by the present invention has excellent charge and discharge capacity, energy density and capacity retention rate. Boron-doped sodium positive electrode materials are single crystals, which have fewer grain boundaries than polycrystalline materials, reducing the generation of cracks during the cycle. At the same time, the single crystals are large in size and small in specific surface area, reducing the contact area between the crystal and the electrolyte, thereby inhibiting the occurrence of some side reactions. Boron elements are easily incorporated into the material lattice without introducing other impurities. The preparation process is simple, efficient and pollution-free. The specific amount of boron source can achieve a balance between the compaction density and the energy density of the positive electrode material. When the amount of boron source is too high, although the compaction density is greatly improved, the capacity will be seriously reduced, which is not conducive to the improvement of energy density. When the amount of boron source is too low, although the impact on the capacity is small, the improvement of the compaction density is also minimal. Therefore, it is necessary to select a suitable boron doping amount to balance the reduction in capacity and the increase in compaction density after boron doping, so that the battery that ultimately protects the positive electrode material has an excellent capacity retention rate.

[0049] 2. The specific coating agent in the present invention can form a coating layer on the surface of the positive electrode material, reduce the contact between the material and the electrolyte, and thus improve the cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0051] Figure 1 Example 1 Electron microscope image of a boron-doped sodium cathode material single crystal;

[0052] Figure 2 XRD spectrum of boron-doped sodium positive electrode material in Example 1;

[0053] Figure 3 Electron microscope image of the sodium battery positive electrode material single crystal of Comparative Example 1. DETAILED DESCRIPTION

[0054] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0055] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0056] Example 1

[0057] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0058] S1. Mix NiSO4, FeSO4 and MnSO4 with water for the first time to obtain a mixed solution, wherein the molar ratio of the metal elements in NiSO4, FeSO4 and MnSO4 is 0.33:0.33:0.33, and the concentration of the metal salt solution in the mixed solution is 3 mol / L; conduct a coprecipitation reaction with the obtained mixed solution, 20 wt% ammonia water and 30 wt% NaOH solution, the flow rate of the mixed solution is 6 L / h, the pH of the reaction system is 12, the ammonia concentration of the reaction system is 8 g / L, nitrogen is introduced, the gas flow rate is 6 L / min, the reaction temperature is 65°C, the reaction time is 15 h, and the product is filtered, washed and dried to obtain Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 precursor;

[0059] S2, according to Na element and Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 Weigh sodium carbonate and Ni (OH)2 precursor in a 1:1 molar ratio 1 / 3 Fe 1 / 3Mn 1 / 3 (OH)2 precursor, Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 Based on the total molar amount of metal elements in the (OH)2 precursor, 0.5 mol% B2O3 was weighed to make the amount of boron element 1 mol%, and the second mixing was carried out. In an air atmosphere, the temperature was first increased to 800°C at a heating rate of 2°C / min and sintered for 4h, and then increased to 1050°C at a heating rate of 2°C / min and sintered for 10h. After natural cooling, the product was crushed and sieved to obtain NaNi 1 / 3 Fe 1 / 3 Mn1 / 3 B 0.01 O2-burning products;

[0060] S3, NaNi obtained by adding S2 1 / 3 Fe 1 / 3 Mn 1 / 3 B 0.01 O2-burning products, NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 B 0.01 The mass of the O2-sintered product was taken as the basis, the amount of ZrO2 was 1wt%, and the temperature was raised to 600℃ at a heating rate of 2℃ / min in air atmosphere for 6h, then cooled to room temperature, and the ZrO2-coated NaNi was obtained after iron removal through sieving. 1 / 3 Fe 1 / 3 Mn 1 / 3 B 0.01 O2 second firing product, i.e. boron-doped sodium positive electrode material, morphology is shown in Figure 1 ,from Figure 1 It can be seen that the prepared boron-doped sodium cathode material is a single crystal morphology, and the XRD spectrum is shown in Figure 2 ,from Figure 2 It can be seen that the boron-doped sodium cathode material is a standard O3 phase, and no other impurities are introduced except for a slight NiO impurity phase.

[0061] Example 2

[0062] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0063] S1, following the steps of S1 in Example 1;

[0064] S2, compared with Example 1, the difference is that Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 Based on the total number of moles of metal elements in the (OH)2 precursor, 1 mol% of B2O3 was weighed so that the amount of boron element in it was 2 mol%;

[0065] S3. Follow the steps of S3 in Example 1.

[0066] Example 3

[0067] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0068] S1, following the steps of S1 in Example 1;

[0069] S2, compared with Example 1, the difference is that according to the Na element and Ni 1 / 3 Fe 1 / 3 Mn1 / 3 Weigh sodium carbonate and Ni (OH)2 precursor in a molar ratio of 0.9:1 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 precursor;

[0070] S3. Follow the steps of S3 in Example 1.

[0071] Example 4

[0072] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0073] S1. Mix NiSO4, FeSO4 and MnSO4 with water for the first time to obtain a mixed solution, wherein the molar ratio of the metal elements in NiSO4, FeSO4 and MnSO4 is 0.4:0.2:0.4, and the concentration of the metal salt solution in the mixed solution is 3.5 mol / L; conduct a coprecipitation reaction with the obtained mixed solution, 25 wt% ammonia water and 25 wt% NaOH solution, the flow rate of the mixed solution is 6 L / h, the pH of the reaction system is 12.2, the ammonia concentration of the reaction system is 7 g / L, nitrogen is introduced, the gas flow rate is 7 L / min, the reaction temperature is 60°C, the reaction time is 12 h, and the product is filtered, washed and dried to obtain Ni 0.4 Fe 0.2 Mn 0.4 (OH)2 precursor;

[0074] S2, according to Na element and Ni 0.4 Fe 0.2 Mn 0.4 Weigh sodium carbonate and Ni with a molar ratio of (OH)2 of 0.95:1 0.4 Fe 0.2 Mn 0.4 (OH)2 precursor, Ni 0.4 Fe 0.2 Mn 0.4 Based on the total molar amount of metal elements in the (OH)2 precursor, 1 mol% H3BO3 was weighed to make the amount of boron element 1 mol%, and the second mixing was performed. In an air atmosphere, the temperature was first increased to 850°C at a heating rate of 3°C / min and sintered for 5h, and then increased to 1020°C at a heating rate of 3°C / min and sintered for 12h. After cooling naturally, the product was crushed and sieved to obtain Na 0.95 Ni 0.4 Fe 0.2 Mn 0.4 B 0.01 O2-burning products;

[0075] S3, add Na obtained from S1 0.95 Ni0.4 Fe 0.2 Mn 0.4 B 0.01 O2-burning products, with Na 0.95 Ni 0.4 Fe 0.2 Mn 0.4 B 0.01 The amount of ZrO2 was 0.5wt% and the temperature was raised to 700℃ at a heating rate of 5℃ / min in air atmosphere for 5h. Then the mixture was cooled to room temperature and iron was removed by sieving to obtain ZrO2-coated Na 0.95 Ni 0.4 Fe 0.2 Mn 0.4 B 0.01 O2 second fired product, that is, boron-doped sodium positive electrode material.

[0076] Example 5

[0077] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0078] S1, following the steps of S1 in Example 1;

[0079] S2, compared with Example 1, the difference is that "1050°C" is changed to "1000°C";

[0080] S3. Follow the steps of S3 in Example 1.

[0081] Example 6

[0082] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0083] S1, following the steps of S1 in Example 1;

[0084] S2, compared with Example 1, the difference is that "sintering at 1050°C for 10h" is changed to "sintering at 1050°C for 14h";

[0085] S3. Follow the steps of S3 in Example 1.

[0086] Example 7

[0087] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0088] S1, following the steps of S1 in Example 1;

[0089] S2. Compared with Example 1, the difference is that “firstly heating to 800°C at a heating rate of 2°C / min and sintering for 4h, then heating to 1050°C at a heating rate of 2°C / min and sintering for 10h” is changed to “firstly heating to 800°C at a heating rate of 5°C / min and sintering for 4h, then heating to 1050°C at a heating rate of 5°C / min and sintering for 10h”;

[0090] S3. Follow the steps of S3 in Example 1.

[0091] Example 8

[0092] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0093] S1, following the steps of S1 in Example 1;

[0094] S2, following the steps of S2 in Example 1;

[0095] S3. Compared with Example 1, the difference is that "ZrO2" is changed to "Al2O3".

[0096] Example 9

[0097] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0098] S1, following the steps of S1 in Example 1;

[0099] S2, following the steps of S2 in Example 1;

[0100] S3. Compared with Example 1, the difference is that "ZrO2" is changed to "CaO".

[0101] Example 10

[0102] This embodiment provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0103] S1, following the steps of S1 in Example 1;

[0104] S2, following the steps of S2 in Example 1;

[0105] S3. Compared with Example 1, the difference is that "600°C" is changed to "800°C".

[0106] Comparative Example 1

[0107] This comparative example provides a method for preparing a positive electrode material, comprising the following steps:

[0108] S1, following the steps of S1 in Example 1;

[0109] S2, compared with Example 1, the difference is that no B2O3 is added;

[0110] S3, following the steps of S3 in Example 1;

[0111] Appearance Figure 3 ,from Figure 3 It can be seen that the sodium positive electrode material prepared in Comparative Example 1 is a single crystal morphology, but the size of the single crystal is relatively small. After adding the B element in Example 1, the size of the single crystal of the sodium positive electrode material prepared is significantly increased.

[0112] Comparative Example 2

[0113] This comparative example provides a method for preparing a positive electrode material, comprising the following steps:

[0114] S1, following the steps of S1 in Example 1;

[0115] S2, compared with Example 1, the difference is that 10 mol% of B2O3 is weighed so that the amount of boron element therein is 20 mol%;

[0116] S3. Follow the steps of S3 in Example 1.

[0117] Comparative Example 3

[0118] This comparative example provides a method for preparing a positive electrode material, comprising the following steps:

[0119] S1, following the steps of S1 in Example 1;

[0120] S2, compared with Example 1, the difference is that 0.05 mol% of B2O3 is weighed so that the amount of boron element therein is 0.1 mol%;

[0121] S3. Follow the steps of S3 in Example 1.

[0122] Comparative Example 4

[0123] This comparative example provides a method for preparing a boron-doped sodium positive electrode material, comprising the following steps:

[0124] S1, following the steps of S1 in Example 1;

[0125] S2, compared with Example 1, the difference is that according to the Na element and Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 Weigh sodium carbonate and Ni (OH)2 precursor in a molar ratio of 0.6:1 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 precursor;

[0126] S3. Follow the steps of S3 in Example 1.

[0127] Comparative Example 5

[0128] This comparative example provides a method for preparing a positive electrode material, comprising the following steps:

[0129] S1, following the steps of S1 in Example 1;

[0130] S2, following the steps of S2 in Example 1;

[0131] The S3 step is not performed.

[0132] Test Case

[0133] The D50 of boron-doped sodium cathode material was tested using a laser particle size tester.

[0134] The compaction density of the positive electrode material was tested using a powder compaction density meter with a test pressure of 13 kN.

[0135] The material prepared in the example or comparative example is used as the positive electrode active material and slurried with polyvinylidene fluoride and carbon black in a ratio of 95:2.5:2.5. The compacted density of the electrode is 3.2 g / cm 3 , made into pole pieces, using metal lithium sheets as counter electrodes, glass fiber as separators, and 1 mol / L lithium hexafluorophosphate ethylene carbonate (EC) and dimethyl carbonate (DMC) solutions (the volume ratio of EC to DMC is 1:1) as electrolytes, assembled into CR2032 button cells in an argon-filled glove box, and finally placed the batteries in a blue-electric test system for electrical performance testing.

[0136] Energy density (ED) test: At room temperature, charge to 4.0V at a constant current with a charge rate of 0.1C, then discharge to 2.0V at a discharge rate of 0.1C to obtain the discharge capacity and average discharge voltage platform; then, according to the actual size (length, width, thickness) of the battery

[0137]

[0138] The electrical performance test conditions are as follows: the cycle test charge and discharge voltage range is 2.0V-4.0V, the test temperature is 25℃, after the open circuit voltage is stable, the battery's initial charge and discharge performance is tested by 0.1C / 0.1C cycle for 1 week, the initial charge capacity is charged at 0.1C constant current until the voltage reaches 4.0V, and the capacity when the current is discharged at 0.1C constant current until the cut-off voltage reaches 2.0V is taken as the initial discharge capacity. Then, 50 cycles of charge and discharge tests are carried out at a rate of 1C / 1C between 2.0-4.0V to characterize the capacity retention rate of the positive electrode material after 50 cycles;

[0139] The specific results are shown in Table 1.

[0140] Table 1

[0141]

[0142] The battery comprising the positive electrode material of the present invention has good electrical performance.

[0143] By comparing Example 1, Comparative Example 2 and Comparative Example 3, it can be seen that in Comparative Example 2, excessive boron is added. Although the positive electrode material obtained has a higher crystal size and compaction density, the capacity of the battery is greatly reduced and the electrical performance is poor; in Comparative Example 3, insufficient boron is used. Although it has excellent charge and discharge capacity, the compaction density is low and the capacity retention rate of the battery finally obtained is also low.

[0144] Comparison between Example 1 and Comparative Example 5 shows that step S3 is not performed in Comparative Example 5. Although the charge and discharge performance is good during the initial use, the capacity retention rate is the lowest after 50 cycles, the stability is poor, and the long-term use is unacceptable, resulting in poor practicality.

[0145] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a boron-doped sodium positive electrode material, characterized in that: The specific steps of the preparation method include: S1. Preparation of Ni a Fe b Mn c (OH)2 precursor; S2, sodium source, boron source, Ni a Fe b Mn c The (OH)2 precursor is mixed for the first time and sintered for the first time to obtain Na x Ni a Fe b Mn c B y O2-burning products; Among them, Ni a Fe b Mn c The amount of boron in the boron source is 0.2-5 mol%, based on the total molar amount of metal elements in the (OH)2 precursor; The sodium element in the sodium source and Ni a Fe b Mn c The molar ratio of (OH)2 precursor is 0.65-1.1:1; S3, the Na x Ni a Fe b Mn c B y The O2-fired product and the coating agent are mixed for the second time and sintered for the second time to obtain a boron-doped sodium positive electrode material.

2. The preparation method according to claim 1, characterized in that: In S2, Ni a Fe b Mn c Based on the total molar amount of metal elements in the (OH)2 precursor, the amount of boron element in the boron source is 0.5-2 mol%.

3. The preparation method according to claim 1 or 2, characterized in that: In S2, the sodium source includes at least one of sodium carbonate and sodium hydroxide; And / or, the boron source includes at least one of boron oxide and boric acid.

4. The preparation method according to any one of claims 1 to 3, characterized in that: In S2, the specific process of the first sintering includes: firstly heating the temperature to 500-850°C at a heating rate of 1-5°C / min and sintering for 2-6h, and then heating the temperature to 900-1200°C at a heating rate of 1-5°C / min and sintering for 5-15h.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In S3, the coating agent includes at least one of a metal oxide and / or a metal salt; Optionally, the metal oxide includes at least one of ZrO2, B2O3, Al2O3, CaO, TiO2, MgO, CoO, MnO, and MnO2; Optionally, the metal salt includes at least one of chloride, bromide, iodide, nitrate and sulfate; Optionally, the chloride salt includes at least one of ZrCl4, AlCl3, CaCl2, TiCl4, MgCl2, CoCl2, and MnCl2; Optionally, the bromide salt includes at least one of ZrBr4, AlBr3, CaBr2, TiBr4, MgBr2, CoBr2, and MnBr2; Optionally, the iodide salt includes at least one of ZrI4, AlI3, CaI2, TiI4, MgI2, CoI2, and MnI2; Optionally, the nitrate includes at least one of Zr(NO3)4, Al(NO3)3, Ca(NO3)2, Ti(NO3)2, Mg(NO3)2, Co(NO3)2, and Mn(NO3)2; Optionally, the sulfate includes at least one of ZrSO4, Al2(SO4)3, MgSO4, CoSO4, and MnSO4; and / or, Na x Ni a Fe b Mn c B y Based on the mass of the O2-sintered product, the amount of the coating agent is 0.3-2wt%.

6. The preparation method according to any one of claims 1 to 5, characterized in that: In S3, the specific process of the second sintering includes: heating to 250-900°C at a heating rate of 1-5°C / min and sintering for 3-8h.

7. The preparation method according to any one of claims 1 to 6, characterized in that: In S1, Ni a Fe b Mn c The specific process of the (OH)2 precursor includes: mixing a nickel source, an iron source, a manganese source and water to obtain a mixed solution, mixing the mixed solution, a complexing agent and a pH regulator, and performing a coprecipitation reaction to obtain Ni a Fe b Mn c (OH)2 precursor; Optionally, the molar ratio of the nickel element in the nickel source, the iron element in the iron source, and the manganese element in the manganese source is (0.2-0.5):(0.2-0.5):(0.2-0.5); Optionally, in the mixed solution, the concentration of the metal salt solution is 3-3.5 mol / L; Optionally, the nickel source includes at least one of nickel sulfate, nickel chloride, nickel carbonate and nickel acetate; Optionally, the iron source includes at least one of ferric sulfate, ferric chloride, ferric carbonate and ferric acetate; Optionally, the manganese source includes at least one of manganese sulfate, manganese chloride, manganese carbonate and manganese acetate.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The coprecipitation reaction temperature is 55-65°C and the time is 8-15h; and / or, when the mixed solution is added, the flow rate of the mixed solution is 5-6 L / h; And / or, in the solution where the coprecipitation reaction occurs, the pH value is 12-12.3, and the concentration of the complexing agent is 8-10 g / L.

9. A boron-doped sodium positive electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. A secondary battery, characterized in that: The secondary battery comprises the boron-doped sodium positive electrode material according to claim 9.