Gradient active mixed material as well as preparation method and application thereof

By preparing shield dry soil with sodium hydroxide concentration gradient and performing rapid calcination at low temperature, the problems of fluctuations in activity index and poor early hardening performance of shield dry soil are solved, and the high activity and stable structure of the mixed material are achieved, satisfying the satisfaction of The performance requirements of high-strength concrete.

CN118930091AActive Publication Date: 2024-11-12HUNAN UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411113170.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The activity index of mixed materials prepared by existing shield dry soil is prone to fluctuation, and the mechanical properties of early hardening slurries are poor, making it difficult to maintain better potential hydraulic properties.

Method used

By preparing shield dry soil with a concentration gradient of sodium hydroxide, it is rapidly calcined at low temperature, destroying the crystal lattice, forming a differential defect structure, promoting the synergistic effect of shield dry soil in the hydration process, and regulating its potential hydraulic stiffness.

Benefits of technology

It significantly improves the early and late activity of the mixed materials, realizes the deep optimization and modification of shield dry soil, meets the performance needs of industries such as high-strength concrete, and ensures the continuous improvement of the slurry structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992874280000071
    Figure BDA0004992874280000071
  • Figure BDA0004992874280000081
    Figure BDA0004992874280000081
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and discloses a gradient active mixed material and a preparation method and application thereof. The preparation method comprises the following steps: preparing at least two parts of first raw materials; the first raw materials are obtained by doping sodium hydroxide solutions into dried shield dried soil and sequentially mixing, stirring, grinding and drying, and the sodium hydroxide contents in the sodium hydroxide solutions doped with the first raw materials are different from one another; mixing the first raw materials according to a preset proportion to obtain a second raw material; calcining the second raw material in an environment at 500-680 DEG C until the surface sodium element is completely reacted, and quenching after calcining to obtain clinker; and grinding the clinker to obtain the gradient active mixed material. According to the embodiment of the invention, the potential hydraulicity of the gradient active admixture can be excited, and the early activity of the gradient active admixture is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of building materials, and in particular to a gradient active mixed material, a preparation method thereof and an application thereof. Background Art

[0002] Admixtures refer to artificial or natural mineral materials that are added to the mill together with clinker and gypsum when grinding cement to improve cement properties, adjust cement grade, and increase cement production.

[0003] In the related art, shield-dried soil can be used to prepare mixed materials, specifically, shield-dried soil is used as raw material, an appropriate amount of alkali is added, and the mixed material is prepared by calcination. However, when shield-dried soil is used to prepare mixed materials, the activity index of the prepared mixed materials is very easy to fluctuate, and it is difficult to always maintain a good potential hydraulic hardness. The potential hydraulic hardness is slow to play, especially the mechanical properties of the early hardened slurry are poor. Summary of the invention

[0004] The purpose of the present application is to provide a gradient active admixture, a preparation method and application thereof, which can stimulate the potential hydraulic hardness of the admixture and improve the early activity of the admixture.

[0005] The present application provides a method for preparing a gradient active mixed material, comprising:

[0006] preparing at least two first raw materials; the first raw materials are obtained by adding sodium hydroxide solution to dry shield-dried soil and then mixing, stirring, grinding and drying in sequence, and the sodium hydroxide content in the sodium hydroxide solution added to each of the first raw materials is different from each other;

[0007] Mixing the first raw materials according to a preset ratio to obtain a second raw material;

[0008] The second raw material is calcined in an environment of 500-680° C. until the surface sodium element is completely reacted, and then rapidly cooled after the calcination to obtain clinker;

[0009] The clinker is ground to obtain a gradient active mixed material.

[0010] Preferably, the mass of the sodium hydroxide solution is 15-25wt% of the mass of the shield dried soil, the mass of the sodium hydroxide added to at least one of the first raw materials is 0.01-1.0wt% of the mass of the shield dried soil, and the mass of the sodium hydroxide added to at least one of the first raw materials is 1.0-12wt% of the mass of the shield dried soil.

[0011] Preferably, the mixing ratio of the first raw material with the highest sodium hydroxide content is 5-50%.

[0012] Preferably, the specific surface area of ​​the first raw material is 360-460m 2 / kg.

[0013] Preferably, the specific surface area of ​​the gradient active mixed material is 360-460m 2 / kg.

[0014] Preferably, the mass of the sodium hydroxide in the second raw material is 0.06-6.5wt% of the mass of the shield drying soil.

[0015] Preferably, the duration of calcining the second raw material is 20-50 minutes.

[0016] Preferably, the rapid cooling is water cooling, and drying is performed after the rapid cooling, and the water temperature of the rapid cooling is not higher than 30°C.

[0017] The embodiments of the present application also provide a gradient active mixed material prepared by the method for preparing the gradient active mixed material as described above.

[0018] The embodiments of the present application also provide the use of the gradient active admixture as described above in the preparation of cement or concrete.

[0019] Beneficial effects of this application:

[0020] (1) A method for preparing a gradient active admixture from shield-dried soil is provided, wherein a sodium hydroxide distribution with a concentration gradient is formed on the surface of the shield-dried soil, and then low-temperature rapid calcination is performed with the help of the sodium element's fluxing, lattice destruction, and liquid phase generation, so that shield-dried soil with different sodium hydroxide concentrations produces different defect structures during the alkali calcination and migration process. Thus, shield-dried soil with different activities can produce a synergistic effect during the hydration process and continuously improve the slurry structure. By adjusting the preparation process parameters, the potential hydraulic hardness of the shield-dried soil at different ages can be regulated and matched to meet the performance requirements of industries such as silicate cement and high-strength concrete for admixtures.

[0021] (2) The shield drying soil with a sodium hydroxide concentration gradient on the calcined surface is used to greatly increase the amount of alkali in the shield drying soil. Not only is the shield drying soil deeply optimized and modified with the help of high alkali, and has extremely high potential hydraulic hardness, but the unreacted sodium hydroxide in the high-alkali shield drying soil will migrate to the low-alkali shield drying soil during the calcination process. The migrated alkali not only modifies and calcines the shield drying soil well, making the shield drying soil have gradient activity, but also effectively reduces the final residual alkali content, making the mixed material extremely active in both the early and late stages. DETAILED DESCRIPTION

[0022] The present application will be further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0023] It should be noted that the terms "first", "second" and the like in the specification and claims are used to distinguish similar objects, but are not used to describe a specific order or sequence.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.

[0025] The present application provides a method for preparing a gradient active mixed material, comprising:

[0026] At least two first raw materials are prepared; the first raw materials are obtained by adding sodium hydroxide solution to dry shield-dried soil and then mixing, stirring, grinding and drying in sequence, and the contents of sodium hydroxide in the sodium hydroxide solutions added to the first raw materials are different from each other;

[0027] Mixing the first raw materials according to a preset ratio to obtain a second raw material;

[0028] The second raw material is calcined in an environment of 500-680°C until the surface sodium element is completely reacted, and then rapidly cooled after the calcination to obtain clinker;

[0029] The clinker is ground to obtain a gradient active mixed material.

[0030] Preferably, the mass of the sodium hydroxide solution is 15-25wt% of the mass of the shield dried soil, the mass of the sodium hydroxide added to the at least one first raw material in the sodium hydroxide solution is 0.01-1.0wt% of the mass of the shield dried soil, and the mass of the sodium hydroxide added to the at least one first raw material in the sodium hydroxide solution is 1.0-12wt% of the mass of the shield dried soil.

[0031] Preferably, the mixing ratio of the first raw meal with the highest sodium hydroxide content is 5-50%.

[0032] Preferably, the specific surface area of ​​the first raw material is 360-460m 2 / kg.

[0033] Preferably, the specific surface area of ​​the gradient active mixed material is 360-460m 2 / kg.

[0034] Preferably, the mass of sodium hydroxide in the second raw material is 0.06-6.5wt% of the mass of shield drying soil.

[0035] Preferably, the duration of calcining the second raw material is 20-50 minutes.

[0036] Preferably, the rapid cooling is water cooling, and drying is performed after the rapid cooling, and the water temperature of the rapid cooling is not higher than 30°C.

[0037] The present application is further described below in conjunction with specific embodiments.

[0038] In the following embodiments and comparative examples, except comparative example 3, two portions of the first raw material are prepared.

[0039] In the following embodiments and comparative examples, the shield drying soil is mixed with 55.4wt% silicon dioxide, 27.8wt% aluminum oxide, 6.3wt% ferrosoferric oxide, 3.2wt% potassium oxide, 2.1wt% magnesium oxide, 1.3wt% titanium dioxide, 2.0wt% calcium oxide, 1.3wt% sodium oxide and 0.6wt% impurities.

[0040] Example 1

[0041] Take 10g of sodium hydroxide and 200.0g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix it and grind it to a specific surface area of ​​400m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​400m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0042] The mixing ratio of the first raw material A and B is set to 50:50. 500g of the first raw material A and 500g of the first raw material B are mixed evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 450°C and calcined for 50 minutes until the sodium element on the surface of the shield drying soil is completely consumed to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​400m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for concrete admixture performance testing is used to test the admixture activity index according to GB / T12957-2005 standard. Referring to Table 1, the admixture activity indexes at 7d and 28d are both high.

[0043] Example 2

[0044] Take 50g of sodium hydroxide and 200.0g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix and grind to a specific surface area of ​​360m 2 / kg, and after drying, a powdered first raw material A is obtained. 5g of sodium hydroxide and 200g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​360m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0045] The mixing ratio of the first raw material A and B is set to 20:80. Take 200g of the first raw material A and 800g of the first raw material B and mix them evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 550℃ and calcined for 30 minutes until the sodium element on the surface of the shield drying soil is completely consumed to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​360m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for concrete admixture performance testing is used to test the admixture activity index according to GB / T12957-2005 standard. Refer to Table 1, the admixture 7d and 28d activity indexes are both very high.

[0046] Example 3

[0047] Take 120g of sodium hydroxide and 250.0g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix and grind to a specific surface area of ​​460m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​460m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0048] The mixing ratio of the first raw material A and B is set to 5:95. Take 50g of the first raw material A and 950g of the first raw material B and mix them evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 650℃ and calcined for 20 minutes until the sodium element on the surface of the shield drying soil is completely consumed to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​460m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for concrete admixture performance testing is used to test the admixture activity index according to GB / T12957-2005 standard. Referring to Table 1, the admixture activity indexes at 7d and 28d are both high.

[0049] Example 4

[0050] Take 50g of sodium hydroxide and 200g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix and grind to a specific surface area of ​​440m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​440m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0051] The mixing ratio of the first raw material A and B is set to 15:85. 150g of the first raw material A and 850g of the first raw material B are mixed evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 650℃ and calcined for 40 minutes until the sodium element on the surface of the shield drying soil is completely consumed to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​440m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for concrete admixture performance testing is used to test the admixture activity index according to GB / T12957-2005 standard. Referring to Table 1, the 7d activity index of the admixture is as high as 98.9%, close to the benchmark cement, and the 28d activity index is as high as 100.2%, exceeding the benchmark cement.

[0052] Comparative Example 1

[0053] Take 50g of sodium hydroxide and 200g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix it and grind it to a specific surface area of ​​450m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​440m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0054] The mixing ratio of the first raw material A and B is set to 80:20. 800g of the first raw material A and 200g of the first raw material B are mixed evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 500°C and calcined for 30 minutes until the sodium element on the surface of the shield drying soil is completely consumed to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​450m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for testing the performance of concrete admixtures is used to test the activity index of the admixture according to GB / T12957-2005 standard. Referring to Table 1, the activity index is unqualified (<65%).

[0055] Comparative Example 2

[0056] Take 300g of sodium hydroxide and 250g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix it and grind it to a specific surface area of ​​420m 2 / kg, and dried to obtain the first raw material A in powder form. Take 0.5g of sodium hydroxide and 150g of water to prepare a sodium hydroxide solution, add it to 1000g of shield-dried soil, mix it and grind it to a specific surface area of ​​420m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0057] The mixing ratio of the first raw material A and B is set to 25:75. Take 250g of the first raw material A and 750g of the first raw material B and mix them evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 550℃ and calcined for 30 minutes until the sodium element on the surface of the shield drying soil is completely consumed to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​420m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for concrete admixture performance testing is used to test the admixture activity index according to GB / T12957-2005 standard. Referring to Table 1, the activity index is poor, only 65.3% at 7d and only 66.5% at 28d.

[0058] Comparative Example 3

[0059] Take 0.5g of sodium hydroxide and 150g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix and grind to a specific surface area of ​​440m 2 / kg, dried to obtain powdered raw material and calcined in a high-temperature furnace at 650℃ for 30 minutes. The clinker was cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​440m 2 / kg, and the mixed material was obtained. The benchmark cement used for testing the performance of concrete admixtures was used to test the activity index of the mixed material according to GB / T12957-2005 standard. Referring to Table 1, the 7d activity index of the mixed material was not high, only 74.6%, and the 28d activity index was 80.1%.

[0060] Comparative Example 4

[0061] Take 50g of sodium hydroxide and 200g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix it and grind it to a specific surface area of ​​450m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​440m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0062] The mixing ratio of the first raw material A and B is set to 15:85. 150g of the first raw material A and 850g of the first raw material B are mixed evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 300°C and calcined for 50 minutes. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​450m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for testing the performance of concrete admixtures is used to test the activity index of the admixture according to GB / T12957-2005 standard. Referring to Table 1, the activity index is unqualified (<65%).

[0063] Comparative Example 5

[0064] Take 50g of sodium hydroxide and 200g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix it and grind it to a specific surface area of ​​450m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​440m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0065] The mixing ratio of the first raw material A and B is set to 15:85. 150g of the first raw material A and 850g of the first raw material B are mixed evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 600℃ and calcined for 5 minutes to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​450m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for testing the performance of concrete admixtures is used to test the activity index of the admixture according to GB / T12957-2005 standard. Referring to Table 1, the activity index is unqualified (<65%).

[0066] Comparative Example 6

[0067] Take 50g of sodium hydroxide and 200g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix it and grind it to a specific surface area of ​​450m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​440m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0068] The mixing ratio of the first raw material A and B is set to 15:85. Take 150g of the first raw material A and 850g of the first raw material B and mix them evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 650℃ and calcined for 100 minutes to ensure that the sodium element on the surface of the shield drying soil is completely reacted to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​450m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for testing the performance of concrete admixtures is used to test the activity index of the admixture according to GB / T12957-2005 standard. Referring to Table 1, the 7d and 28d activity indexes are significantly lower than those of Example 4, and both are less than 85%.

[0069] Comparative Example 7

[0070] Take 50g of sodium hydroxide and 200g of water to make a sodium hydroxide solution, add it to 1000g of shield drying soil, mix it and grind it to a specific surface area of ​​450m 2 / kg, and after drying, a powdered first raw material A is obtained. 0.5g of sodium hydroxide and 150g of water are taken to prepare a sodium hydroxide solution, which is added to 1000g of shield-dried soil, mixed and ground to a specific surface area of ​​440m 2 / kg, and after drying, a powdery first raw material B is obtained.

[0071] The mixing ratio of the first raw material A and B is set to 15:85. 150g of the first raw material A and 850g of the first raw material B are mixed evenly to obtain the second raw material. The second raw material is placed in a high-temperature furnace at 800°C and calcined for 40 minutes to ensure that the sodium element on the surface of the shield drying soil is fully reacted to obtain clinker. The clinker is cooled to room temperature by water cooling and dried, and ground to a specific surface area of ​​450m 2 / kg, a gradient active admixture is obtained. The benchmark cement used for testing the performance of concrete admixtures is used to test the activity index of the admixture according to GB / T12957-2005 standard. Referring to Table 1, the 7d and 28d activity indexes are significantly lower than those of Example 4, and both are less than 80.0%.

[0072] Table 1

[0073]

[0074]

[0075] As can be seen from Examples 1-4, after low-temperature rapid calcination of shield drying soil with a sodium hydroxide concentration gradient, the high-temperature migration and consumption of sodium hydroxide prompts it to produce a differential defective structure, and shield drying soils of different activities can produce a synergistic effect during the hydration process, generating different amounts of secondary hydration products at different ages (7d, 28d, etc.), and continuously, effectively and stably improving the cement hardened slurry structure. For example, in the designed Example 4, the 7d activity index of the hardened slurry is as high as 98.9%, and the 28d strength even exceeds the benchmark cement. Further, by adjusting the process parameters (sodium hydroxide concentration / first raw material ratio / calcination system, etc.), the potential hydraulic depth of shield drying soil at different ages (7d, 28d, etc.) can be controlled and matched to meet the performance requirements of gradient active admixtures in industries such as silicate cement and concrete. As can be seen from Comparative Example 1, the high-alkali shield drying soil content in the second raw material is too high, resulting in a large amount of residual alkali deteriorating slurry structure, and the activity index is unqualified. It can be seen from Comparative Example 2 that if the concentration of sodium hydroxide in the high-alkali shield drying soil in the first raw material is too high, it will cause local alkali excess, which is not conducive to the development of the slurry structure, and the activity index barely meets the standard. It can be seen from Comparative Example 3 that the 28d activity index (81.4%) of the shield drying soil calcined with a very small amount of alkali (0.05%) is acceptable, but the 7d activity index is low, only 74.6%, which confirms that a small amount of alkali cannot improve the early activity of the hardened slurry. It can be seen from Comparative Examples 4 and 5 that lower calcination temperatures or shorter calcination times cannot effectively cause shield drying soil modification reactions, and unreacted alkali will cause the slurry performance to drop sharply, and the activity index is unqualified. It can be seen from Comparative Examples 6 and 7 that increasing the calcination temperature or extending the calcination time cannot further improve the activity index, and even a downward trend appears. The reason is that the inert minerals formed in the shield drying soil hinder the secondary hydration reaction.

[0076] The exemplary embodiments of the present disclosure are specifically shown and described above. It should be understood that the present disclosure is not limited to the configuration or implementation method described herein; on the contrary, the present disclosure is intended to cover various modifications and equivalent configurations contained within the spirit and scope of the appended claims.

Claims

1. A method for preparing a gradient active mixed material, It is characterized in that include: preparing at least two first raw meals; The first raw material is obtained by adding sodium hydroxide solution to dry shield-dried soil and then mixing, stirring, grinding and drying in sequence, and the sodium hydroxide content in the sodium hydroxide solution added to each of the first raw materials is different from each other; Mixing the first raw materials according to a preset ratio to obtain a second raw material; The second raw material is calcined in an environment of 500-680° C. until the surface sodium element is completely reacted, and then rapidly cooled after the calcination to obtain clinker; The clinker is ground to obtain a gradient active mixed material.

2. The method for preparing the gradient active mixed material according to claim 1, It is characterized in that The mass of the sodium hydroxide solution is 15-25wt% of the mass of the shield-dried soil, the mass of the sodium hydroxide added to at least one of the first raw materials is 0.01-1.0wt% of the mass of the shield-dried soil, and the mass of the sodium hydroxide added to at least one of the first raw materials is 1.0-12wt% of the mass of the shield-dried soil.

3. The method for preparing the gradient active mixed material according to claim 1, It is characterized in that The mixing ratio of the first raw material with the highest sodium hydroxide content is 5-50%.

4. The method for preparing the gradient active mixed material according to claim 1, It is characterized in that The specific surface area of ​​the first raw material is 360-460m 2 / kg.

5. The method for preparing the gradient active mixed material according to claim 1, It is characterized in that The specific surface area of ​​the gradient active mixed material is 360-460m 2 / kg.

6. The method for preparing the gradient active mixed material according to claim 1, It is characterized in that The mass of the sodium hydroxide in the second raw material is 0.06-6.5wt% of the mass of the shield drying soil.

7. The method for preparing the gradient active mixed material according to claim 1, It is characterized in that The duration of calcining the second raw material is 20-50 minutes.

8. The method for preparing the gradient active mixed material according to claim 1, It is characterized in that The rapid cooling is water cooling, and drying is performed after the rapid cooling is completed. The water temperature of the rapid cooling is not higher than 30°C.

9. The gradient active mixed material prepared by the method for preparing the gradient active mixed material according to any one of claims 1 to 8.

10. Use of the gradient active admixture as claimed in claim 9 in the preparation of cement or concrete.

Citation Information

Patent Citations

  • Method for preparing amphiphilic gradient copolymer

    CN101974138A

  • Road pavement material prepared by compounding residue soil and steel slag and method for preparing road pavement material

    CN104278609A

  • Efficient plugging film-forming shield slurry material for rescue and emergency

    CN112110682A

  • Additive for drilling mud, and composition for drilling mud

    JP2005015520A