Aggregate, structural performance concrete containing aggregate and preparation method of structural performance concrete
By using core-shell structural aggregates made of biochar cores and gelled materials, the problems of high carbon emissions and shortage of natural aggregates in the construction industry have been solved, and high-strength, low-carbon emission structural performance concrete has been achieved, and biotechnology has been overcome. The problem of reducing mechanical properties of carbon in concrete.
Patent Information
- Application Number
- CN202410570253.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
The construction industry faces the problems of high carbon emissions and shortage of natural aggregates. Direct use of biochar as a concrete substitute will reduce mechanical properties.
Aggregates with shell-encapsulated structures made of biochar cores and gelled materials/alkali excitation materials are prepared by granulation mechanism, and mixed with the matrix material to prepare structural properties concrete, using core shells Structure improves the strength and carbon storage capacity of aggregates.
The structural performance of concrete with high strength and low carbon emissions is achieved. The carbon storage of aggregate exceeds the carbon emissions during the manufacturing process, reducing the porosity and water absorption of biochar, and improving the mechanical properties of concrete.
Smart Images

Figure CN118930103A_ABST
Abstract
Description
[0001] This application claims priority to U.S. patent application 63 / 501,426, filed on May 11, 2023, the entire contents of which are incorporated herein by reference as if fully set forth herein. Technical Field
[0002] The present invention relates to an aggregate (especially an aggregate containing at least biochar), a structural performance concrete containing the aggregate, and a method for preparing the aggregate and the structural performance concrete. Background Art
[0003] High carbon emissions and shortage of natural aggregates are two issues facing the construction industry. On the one hand, the building and construction sector accounts for 39% of the total global process-related carbon dioxide emissions. On the other hand, the uncontrolled exploitation of natural aggregates has had a profound impact on the ecology and has led to a shortage of natural aggregates for the construction industry. Therefore, the development of carbon reduction and natural aggregate replacement technologies is important to achieve the ambitious carbon neutrality goals and sustainable development of the construction industry.
[0004] Biochar is the light black residue left after the pyrolysis of biomass. Due to its carbon storage function, biochar is a carbon reduction solution suitable for building materials. However, directly using biochar as a cement or aggregate substitute will reduce the mechanical properties of concrete, especially when the amount used exceeds a certain threshold.
[0005] Therefore, an object of the present invention is to provide an aggregate, a structural performance concrete containing the aggregate, and a method for preparing the aggregate and the structural performance concrete to overcome the above-mentioned problems, or at least provide a useful alternative. Summary of the invention
[0006] According to a first aspect of the present invention, there is provided an aggregate comprising a core at least partially made of biochar, and a shell encapsulating the core, wherein the shell is at least partially made of a cementitious material and / or an alkali-activated material.
[0007] According to a second aspect of the present invention, there is provided a structural performance concrete, which comprises at least one aggregate and at least one matrix material, wherein the aggregate comprises a core at least partially made of biochar and a shell encapsulating the core, wherein the shell is at least partially made of a cementitious material and / or an alkali-activated material.
[0008] According to a third aspect of the present invention, there is provided a method for preparing aggregate, the method comprising the step (a) of encapsulating a core at least partially made of biochar with a shell at least partially made of a cementitious material and / or an alkali-activated material.
[0009] According to a fourth aspect of the present invention, there is provided a method for preparing structural performance concrete, the method comprising mixing at least one matrix material with at least one aggregate, the aggregate comprising a core at least partially made of biochar and a shell encapsulating the core, wherein the shell is at least partially made of a cementitious material and / or an alkali-activated material. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Embodiments of the present invention will now be described by way of example with reference to the accompanying drawings, in which: Figure 1a A lot of loose biochar is shown; Figure 1b Shown by Figure 1a The plurality of aggregate particles of the present invention formed from the loose biochar shown; Figure 2 shows a cross-sectional view of the aggregate of the present invention; Figure 3 Schematically shows Figure 1b Calculation of the carbon footprint of aggregates; Figure 4a A number of densified biochars are shown; Figure 4b Shown by Figure 4a A plurality of aggregate particles of the present invention formed from densified biochar; Figure 5 is a schematic diagram showing the densification of loose biochar into densified biochar; Figure 6 shows the particle size distribution of ordinary Portland cement (OPC) and granulated blast furnace slag (GGBS) that can be used to form the aggregate of the present invention; Figure 7 The loose bulk density and apparent density (both in kg / m 3 The relationship between maintenance time (in days) and maintenance time (in days); Figure 8 A graph showing the relationship between the cylinder compressive strength (in MPa) and the curing time (in days) of the aggregate of the present invention; Fig. 9 A graph showing the relationship between the water absorption (in wt%) and the curing time (in days) of the aggregate of the present invention; Fig.10 Schematically illustrates the carbon footprint assessment of 1 ton of aggregate of the present invention; and Fig.11 The structural performance concrete of the present invention is shown. DETAILED DESCRIPTION
[0011] Figure 1a A number of loose biochars 10 are shown, and Figure 1b Shown by Figure 1a The loose biochar 10 forms a core-shell aggregate in the form of particles 12 of the present invention.
[0012] As an example, the following table 1 shows the first embodiment of the method according to the present invention. Figure 1a Formation of loose biochar 10 Figure 1b The composition of the aggregate particles 12 and their corresponding dosage:
[0013] Table 1
[0014] In order to prepare the aggregate particles 12 of the embodiment of the present invention of the above composition, the loose biochar 10 and the cementitious shell material (including ordinary Portland cement (OPC) and granulated blast furnace slag (GGBS)) are first premixed in a granulator (e.g., 100 cm in diameter, 25 cm in depth and 45° inclination angle) at a uniform rotation speed of 15 rpm for 2 minutes. During the continuous rotation of the granulator for another 15 minutes, an appropriate amount of water is sprayed on the material. After the water is sprayed, the granulator continues to rotate for another three (3) minutes to further make the aggregate formed by granulation more dense.
[0015] Curing of newly granulated aggregates at room temperature, constant humidity and sealed conditions. Figure 2 As shown, the aggregate 12 produced from the loose biochar 10 is in the form of a core-shell structured particle having a biochar core 12a encapsulated by a shell 12b formed of OPC and GGBS. In addition to the biochar 10, the core 12a may also include solid waste such as fly ash, slag, recycled concrete fines, and recycled glass.
[0016] Although the weight ratio between the corresponding materials OPC, GGBS, loose biochar 10 and water in Table 1 is about 1:4:0.6:1, the weight ratio between these materials may be 0.75-1.25:3-5:0.45-0.75:0.75-1.25.
[0017] according to Figure 3 The carbon footprint of the aggregate 12 thus formed was calculated, and the results showed that the aggregate 12 made of loose biochar 10 had a carbon footprint of 789 kg / m 3 The biochar 10 has a loose bulk density of 1.2777777, a drum strength of 6.84 MPa, and carbon emissions as low as -69 kgCO2eq / t, where "CO2eq" means "carbon dioxide equivalent". Since the biochar 10 is a carbon storage material, by encapsulating the biochar 10 (with or without solid waste) by the shell 12b, the aggregate 12 is "carbon negative", which means that the amount of carbon stored / encapsulated in the aggregate 12 is greater than the amount of carbon generated in the manufacturing of the aggregate 12, including the carbon emitting raw materials (including OPC, GGBS, water), transportation and pelletizing processes.
[0018] In addition, since the aggregate 12 has the rigid shell 12 b , the aggregate 12 not only overcomes the disadvantages of the biochar 10 due to its high porosity and high water absorption, but also obtains good strength.
[0019] Although in the above-described embodiments, the cementitious shell material includes ordinary Portland cement (OPC) and granulated blast furnace slag (GGBS), other cementitious materials (eg, waste glass powder, recycled powder, silica powder, and incinerator bottom ash (IBA)) may also be used.
[0020] In a second embodiment, densified biochar 14 (such as Figure 4a ) to form a core-shell aggregate 16 in the form of particles (as shown in Figure 4b ). Figure 5 Schematic representation of the densification of loose waste wood biochar into densified / compacted biochar particles, for example by compression. Figure 5 As shown, a plurality of loose waste wood biochar 20 are fed into a compressor 22 and mixed with oil (e.g., motor oil) and sand. The weight ratio of loose biochar 20, oil, and sand may be 7.5-12.5:0.75-1.25:0.75-1.25, such as 10:1:1.
[0021] As the compressor rotates, the loose biochar 20 is mixed with the oil and sand, and is compressed / compacted by the compressor 22, and extruded through multiple outlets, and cut into particles of dense / compacted biochar 26, 28 by the cutter 24, and the outlets have different sizes, so that densified biochar particles 26, 28 of different sizes can be formed. For example, the size of the densified biochar particles 26 is between 2.36mm and 4.75mm, and the size of the densified biochar particles 28 is between 4.75mm and 10mm. It should be noted that the compression method of the loose biochar into the dense biochar is not limited to the one listed above.
[0022] The loose bulk density and apparent density of loose biochar 20, dense / compacted biochar particles 26 with sizes between 2.36 mm and 4.75 mm, and dense / compacted biochar particles 28 with sizes between 4.75 mm and 10 mm are shown in Table 2, respectively.
[0023] Table 2
[0024] The "loose bulk density" of biochar is calculated by dividing the total weight of the biochar by the total volume of the biochar (including the space between and within the biochar particles), and the "apparent density" of biochar is calculated by dividing the total weight of the biochar by the total volume of the biochar (including the space within the biochar particles but excluding the space between the biochar particles).
[0025] Table 3 below shows a second embodiment of the method of the present invention, by cold bonding Figure 4a Densified biochar 14 is formed Figure 4b The ingredients of the aggregate particles 16 and their respective amounts:
[0026] Table 3
[0027] The raw core material (i.e., densified biochar particles 14, 26, 28) and the gelling shell material (OPC and GGBS) were first premixed in a granulator (diameter: 100 cm, depth: 25 cm, and inclination angle: 45°) at a uniform rotation speed of 15 rpm for 2 minutes. During the continuous rotation of the granulator for another 15 minutes, an appropriate amount of water was sprayed on the material. After the water spraying, the granulator was rotated for another 3 minutes to further compact the newly granulated aggregate. The newly granulated aggregate was cured under room temperature, normal humidity and sealed conditions. Figure 4b Aggregate particles 16 based on densified biochar 14, 26, 28 are shown. The aggregate particles 16 have a core-shell structure, each comprising a core of densified biochar (with or without solid waste) enclosing a shell formed of OPC and GGBS.
[0028] For the OPC and GGBS forming the shell, their respective sizes are 1 μm-100 μm, and their respective compositions may be as shown in Table 4.
[0029] Table 4 In Table 4, "LOI" stands for "Loss on Ignition".
[0030] Figure 6 The particle size distribution of OPC (cement) and GGBS used in the above method to form the shell of aggregate 16 is shown. In addition, the apparent density of OPC is 3,100 kg / m 3 The apparent density of GGBS is 2,800 kg / m 3 The apparent density of compacted biochar is 1,338 kg / m 3 .
[0031] according to Fig.10 The carbon footprint of the aggregate particles 16 was calculated and it was found that after 28 days of curing, the aggregate 16 based on densified biochar 14, 26, 28 had a carbon footprint of 878 kg / m 3The aggregate particles 16 have a loose packing density of 1.57 MPa, a drum compressive strength of 7.6 MPa, and carbon emissions as low as -174 kgCO2eq / t. Likewise, the aggregate particles 16 are carbon negative because the amount of carbon stored / encapsulated in the aggregate 16 is greater than the amount of carbon generated when the aggregate 16 is manufactured, including the amount of carbon generated during the manufacture of other materials (including OPC, GGBS, water), transportation, and pelletizing.
[0032] Although the weight ratios of OPC, GGBS, densified biochar, and water in Table 3 are each approximately 10:40:12:1.05, the weight ratios of these materials may be 7.5-12.5:36-44:9-15:0.79-1.31.
[0033] Figure 7 The loose bulk density and apparent density (both in kg / m 3 The relationship between the maintenance time (in days) and the maintenance time (in days). Figure 8 A graph showing the relationship between the cylinder compressive strength (in MPa) of the aggregate particles of the present invention and the curing time (in days), and Fig. 9 A graph showing the water absorption (in wt%) of the aggregate of the present invention versus the curing time (in days) is shown.
[0034] In further embodiments, the densified biochar based aggregate formed from the components shown in Table 5 has higher strength.
[0035] Table 5
[0036] The gelling shell materials (including OPC, GGBS and silica fume) are designed using a modified Andreasen Andersen model to achieve the optimal stacking design. The original core material (including densified biochar) and the shell material are first premixed in a granulator (e.g., diameter 100 cm, depth 25 cm and inclination angle 45°) at a uniform rotation speed of 15 rpm for 2 minutes. During the continuous rotation of the granulator for another 15 minutes, an appropriate amount of water is sprayed on the material. After the water spraying, the granulator is rotated for another 3 minutes to further densify the newly granulated fresh aggregate.
[0037] Thereafter, nanomaterials such as nano-silica are sprayed onto the shell of the aggregate to form a reactive surface, thereby strengthening and promoting the interface between the aggregate and the concrete matrix material when the aggregate is used in concrete production.
[0038] The freshly granulated aggregate was cured under sealed conditions at room temperature and humidity and in a CO2 environment such as 1Pa pressure and 100% CO2 concentration. Carbonization can further improve aggregate strength and reduce carbon emissions. The results showed that the densified biochar-based aggregate with core-shell structure design and sealed curing for 28 days and carbonization for another 6 hours had a cylinder compressive strength of 8.138MPa, showing an increase in strength.
[0039] Table 6 below lists the ingredients for producing structural performance concrete using the densified biochar-based negative carbon aggregate (with a maximum size of 10 mm) shown in Figure 4(b).
[0040] Table 6 Cement (kg) GGBS(kg) Silicon powder Carbon negative aggregate (kg) Water (kg) Additives(kg) 200 340 60 1036 180 10 The admixtures in Table 6 are additives for structural performance concrete, such as superplasticizers (water reducers), fibers, hydroxypropyl methylcellulose (HPMC), etc.
[0041] Although the weight ratio of cement, GGBS, silica fume, negative carbon aggregate, water and admixture in Table 6 is 20:34:6:104:18:1, the ratio may be in the range of 15-25:26-43:4.5-7.5:78-130:13.5-22.5:0.75-1.25.
[0042] Cementitious materials (including cement, GGBS and silica fume) and natural aggregates are designed by the modified Andreasen-Andersen model to achieve optimal packing design. These materials are mixed with water to form a matrix material, and the aggregate of the present invention is added to the matrix material and mixed with the matrix material to form structural performance concrete 30, especially as Fig.11 The cylindrical concrete samples shown have a diameter of 80 mm.
[0043] The results show that the 28d compressive strength of structural performance concrete 30 is higher than 40MPa and the density is less than 1900kg / m 3 And the carbon emission is -7.86kgCO2eq / m 3 , which means that the structural performance concrete 30 is also carbon negative. It should be noted that the structural performance carbon negative concrete can also be designed to have other different densities and different strengths as required.
[0044] Although in the above examples, the cementitious materials include OPC, GGBS, and silica fume, other cementitious materials such as waste glass powder, recycled powder, and incinerator bottom ash (IBA) may also be used.
[0045] Although the shell is made of at least a gelling material in the above-described embodiment, the shell may also be made of an alkali-activated material instead of or in combination with the gelling material. The alkali-activated material may be one or more precursors (e.g., GGBS, fly ash, silica powder, waste glass powder, etc.) activated by an alkali material (e.g., water glass, sodium hydroxide, etc.).
[0046] It should be understood that the above describes only examples in which the present invention may be implemented and that various modifications and / or changes may be made thereto without departing from the spirit of the present invention.
[0047] It should also be understood that, for clarity, certain features of the invention described in separate embodiments may be combined in a single embodiment. Conversely, for brevity, various features of the invention described in a single embodiment may also exist separately or in any suitable sub-combination.
Claims
1. An aggregate, It is characterized in that The aggregate contains: a core made at least in part from biochar, and a shell encapsulating the core, Wherein, the shell is at least partially made of a gelling material and / or an alkali-activated material.
2. The aggregate according to claim 1, in, The cementitious material is at least one of cement, granulated blast furnace slag (GGBS), waste glass powder, recycled powder, silica powder and incinerator bottom ash (IBA).
3. The aggregate according to claim 1, in, The core is a 100 kg / m 3 -300kg / m 3 Loose biochar with a loose bulk density of more than 300 kg / m 3 The loose bulk density of compressed / compacted biochar.
4. The aggregate according to claim 1, in, The shell includes at least one nanomaterial.
5. Aggregate according to claim 4, in, The nano material is silicon powder or nano silicon dioxide.
6. The aggregate according to claim 1, in, The aggregate is carbon negative.
7. The aggregate according to claim 1, in, The aggregate is in the form of particles.
8. A structural performance concrete, It is characterized in that The structural performance concrete comprises at least the aggregate according to any one of claims 1 to 7 and at least one matrix material.
9. The structural performance concrete according to claim 8, in, The matrix material is a gelling material.
10. The structural performance concrete according to claim 8, in, The matrix material includes at least one of cement, GGBS and silica fume.
11. The structural performance concrete according to claim 8, in, The structural performance concrete is carbon negative.
12. The structural performance concrete according to claim 8, in, The 28d compressive strength of the structural performance concrete is at least 30 MPa.
13. A method for preparing aggregate, It is characterized in that The method comprises the step (a): encapsulating a core at least partially made of biochar with a shell at least partially made of a gelling material and / or an alkali-activated material.
14. The method according to claim 13, in, The shell is at least partially made of cement and granulated blast furnace slag (GGBS).
15. The method according to claim 13, in, The method further comprises, before step (a), a step (b) of compacting the biochar to increase its density.
16. The method according to claim 13, in, The method further comprises the step (c) of applying at least one nanomaterial on the shell.
17. The method according to claim 16, in, The nano material is silicon powder or nano silicon dioxide.
18. The method according to claim 13, in, The aggregate is formed by cold bonding.
19. A method for preparing structural performance concrete, It is characterized in that The method comprises mixing at least the aggregate according to one of claims 1 to 7 with at least one matrix material.
20. The method according to claim 19, in, The matrix material is a gelling material.
21. The method according to claim 19, in, The matrix material includes at least one of cement, GGBS, silica powder, waste glass powder, recycled powder and incinerator bottom ash (IBA).
Citation Information
Cited By
Negative carbon lightweight aggregate concrete mix proportion design method and preparation method