High-mud-resistance glue reducing agent and preparation method thereof
The high mud-resistant glue reducing agent designed by polymer structure solves the problem of poor workingability of concrete. The high mud-resistant glue reducing agent designed by polymer structure significantly improves the compressive strength and flowability of concrete. It enhances the dispersion and wrapping properties of concrete and adapts to the stable effect under high mud content.
Patent Information
- Application Number
- CN202411059582.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The problem of poor concrete workingability is mainly due to the degraded quality of sand and gravel and fluctuations in the composition of the glue, resulting in insufficient concrete strength at low glue usage, and existing glue reducing agents cannot effectively solve this problem.
High-resistance mud-type glue reducing agent designed with polymer structure is prepared by combining dispersant, water retention agent and intercalator, which can improve concrete strength and reduce clay impurities on concrete. Adverse effects of quality. The specific method includes preparing polyether monomers, ether substances and carboxy heads in an autoclave to form an intercalator with specific functions to enhance concrete properties.
It significantly improves the compressive strength and fluidity of concrete, enhances the dispersion and wrapping properties of concrete, and maintains a stable effect under high mud content, solving the problem of poor workingability of concrete.
Smart Images

Figure BDA0004977457940000041 
Figure BDA0004977457940000051 
Figure BDA0004977457940000052
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete admixtures, and in particular to a high-mud resistance type gel reducer and a preparation method thereof. Background Art
[0002] Concrete glue reducer is an admixture that reduces the amount of cement without reducing the mechanical properties of concrete. It also improves the workability of concrete and increases the strength at all ages. With the consumption of resources, the quality of sand and gravel decreases, resulting in poor workability of concrete. Maintaining high quality of concrete with low glue dosage is an effective way for concrete production companies to reduce costs, increase efficiency and ensure quality. Therefore, it is of great significance to develop a concrete glue reducer.
[0003] CN115784662A discloses a concrete glue reducer. The glue reducer of the invention comprises the following raw materials in parts by weight: 4-10 parts of organic alcohol amine, 4-6 parts of polycarboxylic acid water reducer, 1-2 parts of early strength component, 0.5-1.5 parts of antifreeze component, 0.03-0.05 parts of water retention and viscosity increasing component, and the balance is water. By adding components such as comb-shaped polycarboxylic acid water reducer and organic alcohol amine, the water consumption of a single cubic meter of concrete can be reduced, the water-cement ratio can be reduced, and the early strength of concrete can be improved.
[0004] CN117843278A discloses a concrete adhesive reducer and its preparation method, which is composed of the following raw materials in parts by weight: 0.5-3% composite microcapsules, 1-5% mesoporous silica, 0.5-4% phase change composition, 0.2-2% polycarboxylic acid copolymer, 15-30% fly ash, 0.1-1% natural organic acid, 0.05-0.5% dispersant, and the balance is water. The invention uses composite microcapsule technology to fill repair agent epoxy resin and polyurethane into microcapsules. When tiny cracks appear in the concrete structure, the cracks are effectively and automatically filled and blocked to improve its compactness and strength. The microencapsulated paraffin absorbs or releases heat when the ambient temperature changes, effectively helping to regulate the internal temperature of the concrete.
[0005] CN116217123A discloses a concrete glue reducer and a preparation method thereof, which is prepared from triethanolamine, triethylenetetramine, triisopropanolamine, salicylic acid, sodium methyl silicate, ethylene glycol, inorganic salt, 2-hydroxyphosphonoacetic acid and water. The glue reducer of the invention is used in a small amount and can increase the strength of concrete, improve the durability of concrete and improve the construction performance of concrete. It is directly added to raw materials such as cement to make concrete, and high-quality concrete products can be obtained after simple stirring, which overcomes the disadvantages of the inconvenience of using the glue reducer and the poor stability of the glue reducer.
[0006] Problems such as reduced sand and gravel quality, large fluctuations in adhesive composition, and insufficient concrete strength at low adhesive dosage lead to poor concrete workability. In view of the above problems, the present invention proposes a high mud resistance type reducer, which solves the problem of the above problems affecting concrete quality through polymer structure design. Summary of the invention
[0007] The invention provides a high-mud resistance type glue reducer and a preparation method thereof. The high-mud resistance type glue reducer provided by the invention can improve the strength of concrete and reduce the adverse effects of clay impurities in concrete on its quality.
[0008] To solve the above problems, the technical solution of the present invention is as follows, and the parts are all parts by mass.
[0009] The high mud resistance type gel reducer of the present invention is prepared by compounding the prepared dispersant, water retaining agent, intercalating agent and polymerized polyol in a mass ratio of 2:1:1:4;
[0010] The dispersant is prepared by 90.13-143.26 parts of amine head, 1.0-2.2 parts of catalyst, 47.72-78.18 parts of cyclic monomer at 120°C to obtain a polyether monomer, and 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water to prepare a liquid A, and 128.97-150.16 parts of ether substance, 3.2-7.9 parts of reducing agent and water to prepare a liquid B to obtain the polyether monomer at 55-65°C.
[0011] The water retaining agent is obtained by polymerizing 104.96 to 185.26 parts of amine heads, 1.0 to 2.2 parts of catalysts, and 114.75 to 195.05 parts of cyclic monomers at 90-120°C;
[0012] The intercalant is obtained by reacting 159.57 to 208.33 parts of carboxyl heads, 1.0 to 2.2 parts of catalysts, and 91.77 to 140.42 parts of cyclic monomers at 130 to 140°C.
[0013] The preparation method of the high mud resistance type glue reducing agent of the present invention is as follows:
[0014] (1) Preparation of dispersant
[0015] Step 1: Add 90.13-143.26 parts of amine heads to a high-pressure reactor, raise the temperature to 120°C while evacuating, and the pressure in the reactor is 0.2-0.3MPa. The materials in the reactor are sucked out from the reactor and then sprayed from the top of the reactor. At the same time, add cyclic monomers. After a period of circulation, cool to 90-100°C, add 1.0-2.2 parts of catalyst, replace with nitrogen, and start evacuating to a gauge pressure of -0.1MPa, and then raise the temperature to 120°C. Start to introduce the remaining cyclic monomers into the reactor, and introduce a total of 47.72-78.18 parts of cyclic monomers into the reactor, control the pressure to be less than 0.4MPa, and keep circulating spray for 2.0-2.5h after all the cyclic monomers are introduced into the reactor. After the reaction is completed, keep warm for 1h to obtain a polyether monomer;
[0016] Step 2: Add the prepared polyether monomer to the reaction kettle, heat it to 55-65°C in a water bath and keep it warm; prepare 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water to make liquid A; prepare 128.97-150.16 parts of ether substance, 3.2-7.9 parts of reducing agent and water to make liquid B; drip liquid A and liquid B at the same time, wherein liquid A is dripped for 2-2.5 hours and liquid B is dripped for 1.5-2 hours; keep the temperature for 1 hour after the dripping of liquid A, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a dispersant mother liquor with a concentration of 30%. The several parts of polyether monomer prepared in step 1 are adjusted in a certain proportion according to the required amount in step 2, so as to control the concentration of the dispersant mother liquor obtained by the reaction to be always controlled at 30%, which reduces the workload for subsequent compounding and other work.
[0017] (2) Preparation of water-retaining agent
[0018] Step 1: Add 104.96-185.26 parts of amine heads into a high-pressure reactor, raise the temperature to 120°C while evacuating, and the pressure in the reactor is 0.2-0.3MPa. The material in the reactor is sucked out from the reactor and then sprayed into the reactor from the top. At the same time, add cyclic monomers. After a period of circulation, cool to 90-100°C.
[0019] Step 2: Add 1.0-2.2 parts of catalyst and replace with nitrogen to start vacuuming to a gauge pressure of -0.1MPa, then raise the temperature to 120°C. Start to introduce the remaining cyclic monomers into the reactor, and introduce a total of 114.75-195.05 parts of cyclic monomers into the reactor, control the pressure to be less than 0.4MPa, and keep circulating spray for 2.0-2.5h after all the cyclic monomers are introduced into the reactor. After the reaction is completed, keep warm for 1h, add 5.9-9.4 parts of neutralizer at one time, and add water to 1000 parts to obtain a mother solution of water retaining agent with a concentration of 30%.
[0020] (3) Preparation of intercalation agent
[0021] 159.57-208.33 parts of carboxyl heads and 1.0-2.2 parts of catalysts are added to a high-pressure reactor. After nitrogen replacement for several times, vacuum is started to be drawn to a gauge pressure of -0.1 MPa, and then the temperature is raised to 130-140°C and maintained for 60 minutes, and then the temperature is raised to 140°C and maintained at this temperature. The reaction pressure is maintained at 0.3 MPa by controlling the introduction rate of cyclic monomers. When the total amount of cyclic monomers introduced is 91.77-140.42 parts, the material is stopped, and a aging reaction is carried out at 140°C until the pressure no longer decreases, and a vacuum treatment is carried out at a pressure of -0.09 MPa for 30 minutes, and then the temperature is reduced to 40°C for discharging, and 5.9-9.4 parts of a neutralizer are added at one time and then water is added to 1000 parts to obtain a mother liquor with a concentration of 30%.
[0022] (4) Preparation of high mud resistance type glue reducer
[0023] The prepared dispersant mother solution, water retaining agent mother solution, intercalating agent mother solution and polymerized polyol are compounded in a mass ratio of 2:1:1:4, and water is added to 1000 parts to obtain the highly anti-mud type gel reducer mother solution with a mass concentration of 50%.
[0024] Preferably, the amine head is 3-(N-allylamino)propyltrimethoxysilane.
[0025] Preferably, the catalyst is one of sodium hydroxide, potassium hydroxide and sodium methoxide, and sodium methoxide is most preferred.
[0026] Preferably, the cyclic monomer is one of ethylene oxide and propylene oxide, and the molar ratio of the cyclic monomer in the dispersant is a mixture of ethylene oxide and propylene oxide in a range of 1 to 6:1, most preferably 2.6:1.
[0027] Preferably, the initiator is one of ammonium persulfate, diisopropyl peroxydicarbonate, and dihexyl peroxydicarbonate, and ammonium persulfate is most preferred; the chain transfer agent is one of thioglycolic acid, mercaptoethanol, and mercaptopropionic acid, and mercaptoethanol is most preferred; and the ether substance is diethylene glycol monoallyl ether or propylene glycol monoallyl ether.
[0028] Preferably, the amine head is N-methyl-allylamine; the reducing agent is sodium hypophosphite; the neutralizing agent is potassium carbonate; and the carboxyl head in the intercalating agent is tiglic acid.
[0029] Preferably, the alcohol-ether ratio is 1.7-2.5:1, most preferably 2.2:1.
[0030] Preferably, the polymeric polyol is composed of several of ethylene glycol, glycerol, trimerpropylene glycol and triethanolamine.
[0031] Preferably, the molar ratio of the dispersant, the water retaining agent, the intercalating agent and the polymeric polyol is 2:1:1:4.
[0032] The present invention is mainly based on the functional design of polymers based on the reaction of the terminal hydroxyl group of the alcohol head with the epoxy monomer. A low molecular weight polymer of about 4000 is synthesized by etherification of the alcohol head and the epoxy group. The epoxy material is selected from ethylene oxide and propylene oxide. The number of methyl groups is adjusted by adjusting the grafting ratio of ethylene oxide and propylene oxide, thereby flexibly changing the viscosity reduction or viscosity increase of the polymer. Different from the water reducer, the adapter does not have an anchoring group to avoid competitive adsorption with other admixtures, or occupying the active sites of the particles, resulting in the water reducer being unable to adsorb and thus failing.
[0033] The molecular weight of the dispersant component is small enough compared to that of traditional water reducers, so that the adaptor can act in the narrow space that the large molecules of the water reducer cannot enter, play a dispersing role, increase the contact area between the particles and water, and accelerate the hydration process; the adsorption capacity of hydroxyl groups is relatively weak, so that the adaptor is in a dynamic process of adsorption-desorption during the hydration process, and will not produce performance sensitivity.
[0034] Based on this structural feature, when the adapter is used in combination with other admixtures, there will be no competitive adsorption phenomenon, and the molecular conformation is small, so it can act on the parts that the water reducer cannot act on, and can effectively improve the performance of cement products.
[0035] The small molecular weight intercalant in the adapter does not have a clearly directional polar group in its structure and will not react with cement particles. Instead, it will intercalate with the impurity clay in the concrete, which can discharge water between the clay layers and prevent the clay from having an adverse effect on the performance of the concrete.
[0036] The beneficial effects of the present invention are as follows:
[0037] 1. The dispersant in the high mud resistance reducing agent provided by the present invention is prepared by reacting the terminal amine group with an epoxide. The amine group can provide a lone pair of electrons to adsorb to the particles, and the ether chain exerts a dispersing effect.
[0038] 2. The viscosity regulator in the machine-made sand regulator provided by the present invention can be adsorbed on the surface of solid particles through the property of the amine group that can give out electron pairs, thereby adjusting the viscosity of the particles.
[0039] 3. The molecular structure of the intercalating agent in the machine-made sand conditioner provided by the present invention contains low-density carbonyl, ether bond, and hydroxyl groups. The carbonyl and ether bonds can be physically adsorbed with clay particles through hydrogen bonds; its molecular conformation is small enough to enter between clay layers and discharge interlayer water. DETAILED DESCRIPTION
[0040] The applicant will further explain the technical solutions and beneficial effects of the present invention in detail in conjunction with specific embodiments, but it should be understood that the following embodiments should not be construed as limiting the scope of protection requested by the claims of this application to any extent.
[0041] The concrete reducer and water reducer prepared in the example are applied to concrete, and compared with the blank example without the reducer and the commercially available reducer (Jiye Changqing reducer), and the cement paste fluidity and cement mortar water reduction rate of the concrete anti-mud agent prepared by the method described in each embodiment and comparative example are tested respectively, and the test method is carried out in accordance with the national standard GB8077-2012 "Concrete admixture homogeneity test method". The concrete anti-mud agent prepared by the method described in the above embodiments and comparative examples is respectively configured into concrete, and the raw material ratio and preparation process are shown in Tables 1 and 2. Concrete is prepared according to the compressive strength test requirements of the national standard GB / T 50081-2019 "Concrete Physical and Mechanical Properties Test Method Standard" standard specimens, cured for 28 days according to the standard requirements, and then the compressive strength of each specimen is tested according to the above standard provisions. The results are shown in Tables 4 and 5.
[0042] Table 1 Raw material composition of high mud resistance type reducer
[0043]
[0044]
[0045] Table 2 Preparation process of high mud resistance type reducer
[0046]
[0047]
[0048] Table 3 Concrete preparation materials
[0049]
[0050] Table 4 Compressive strength test results
[0051]
[0052] Table 5 Concrete fluidity test results
[0053]
[0054]
[0055] The highly mud-resistant anti-mud concrete gel reducer prepared in Examples 1-6 is added to a concrete material with a mud content of 5%, and can still exert a stable effect. This shows that even when the mud content of the concrete raw materials is high, the mud-resistant concrete gel reducer provided by the present invention can still significantly improve the working properties of the concrete, such as strength, fluidity, dispersibility and encapsulation, and has excellent adaptability to mud content and good working effects.
[0056] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high mud resistance type gel reducer, characterized in that: The prepared dispersant, water retaining agent, intercalating agent and polymerized polyol are compounded in a mass ratio of 2:1:1:4, and the following parts are all parts by mass; The dispersant is prepared by preparing a polyether monomer at 120° C. with 90.13 to 143.26 parts of an amine head, 1.0 to 2.2 parts of a catalyst, and 47.72 to 78.18 parts of a cyclic monomer, and simultaneously adding 5.6 to 8.6 parts of an initiator, 1.2 to 4.8 parts of a chain transfer agent, and water to prepare a liquid A, and 128.97 to 150.16 parts of an ether substance, 3.2 to 7.9 parts of a reducing agent, and water to prepare a liquid B to the polyether monomer at 55 to 65° C.; after the reaction, the obtained product is obtained; The water retaining agent is obtained by polymerizing 104.96-185.26 parts of amine head, 1.0-2.2 parts of catalyst, and 114.75-195.05 parts of cyclic monomer at 90-120°C; The intercalant is obtained by reacting 159.57-208.33 parts of carboxyl heads, 1.0-2.2 parts of catalysts, and 91.77-140.42 parts of cyclic monomers at 130-140°C.
2. The method for preparing the highly anti-mud type adhesive reducer according to claim 1, characterized in that The parts mentioned are all parts by mass. The following steps are involved: (1) Preparation of dispersant Step 1: Add 90.13-143.26 parts of amine heads to a high-pressure reactor, vacuumize and heat to 120°C, the pressure in the reactor is 0.2-0.3MPa, the materials in the reactor are sucked out from the reactor and then sprayed from the upper part of the reactor, and cyclic monomers are added at the same time, and the reactor is cooled to 90-100°C, 1.0-2.2 parts of catalyst are added, and the pressure is replaced with nitrogen and vacuumized to a gauge pressure of -0.1MPa, and the temperature is raised to 120°C, and the remaining cyclic monomers are introduced into the reactor. A total of 47.72-78.18 parts of cyclic monomers are introduced into the reactor, and the pressure is controlled to be less than 0.4MPa. After all the cyclic monomers are introduced into the reactor, the circulating spray is maintained for 2.0-2.5h, and the reaction is kept warm for 1h; Step 2: Add the polyether monomer obtained in step 1 to the reaction kettle, heat it to 55-65°C in a water bath and then keep it warm; prepare liquid A by adding 5.6-8.6 parts of initiator, 1.2-4.8 parts of chain transfer agent and water; prepare liquid B by adding 128.97-150.16 parts of ether substance, 3.2-7.9 parts of reducing agent and water; add liquid A and liquid B at the same time, wherein liquid A is added for 2-2.5 hours and liquid B is added for 1.5-2 hours; after adding liquid A, keep it warm for 1 hour, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a dispersant mother solution with a concentration of 30wt%; (2) Preparation of water-retaining agent Step 1: Add 104.96~185.26 parts of amine head into the autoclave, raise the temperature to 120℃ while evacuating, the pressure in the autoclave is 0.2~0.3MPa, the material in the autoclave is sucked out from the autoclave and then sprayed into the autoclave from the top, and the cyclic monomer is added at the same time. After a period of circulation, cool to 90~100℃; Step 2: Add 1.0-2.2 parts of catalyst and replace with nitrogen to start vacuuming to a gauge pressure of -0.1 MPa, then raise the temperature to 120°C, start introducing the remaining cyclic monomer into the reactor, introduce a total of 114.75-195.05 parts of cyclic monomer into the reactor, control the pressure to be less than 0.4 MPa, maintain circulating spraying for 2.0-2.5 hours after all the cyclic monomers are introduced into the reactor, keep warm for 1 hour after the reaction is completed, add 5.9-9.4 parts of neutralizer at one time and add water to 1000 parts to obtain a defect inducing agent mother liquor with a concentration of 30wt%; (3) Preparation of intercalation agent 159.57-208.33 parts of carboxyl head and 1.0-2.2 parts of catalyst were added to the autoclave, and after nitrogen replacement for several times, vacuum was started to be drawn to a gauge pressure of -0.1 MPa, and then the temperature was raised to 130-140°C and maintained for 60 minutes, and then the temperature was raised to 140°C and maintained at this temperature, and the reaction pressure was kept at 0.3 MPa by controlling the introduction rate of the cyclic monomer, and the introduction of the material was stopped when the total amount of the cyclic monomer introduced was 91.77-140.42 parts, and the aging reaction was carried out at 140°C until the pressure no longer decreased, and vacuum treatment was carried out at a pressure of -0.09 MPa for 30 minutes, and then the temperature was lowered to 40°C for discharging, and 5.9-9.4 parts of a neutralizer were added at one time and then water was added to 1000 parts to obtain a mother liquor with a concentration of 30%; (4) Preparation of high mud resistance type reducer The prepared dispersant mother liquor, water retaining agent mother liquor, intercalating agent mother liquor and polymerized polyol are compounded in a certain proportion and water is added to 1000 parts to obtain the high mud resistance type reducer mother liquor with a concentration of 50%. The high mud resistance type reducer mother liquor is diluted at 1:29 to obtain the high mud resistance type reducer working fluid, and its usage dosage is 0.5%.
3. The method according to claim 2, characterized in that The amine head is 3-(N-allylamino)propyltrimethoxysilane.
4. The method according to claim 2, characterized in that: The catalyst is one of sodium hydroxide, potassium hydroxide and sodium methoxide.
5. The method according to claim 2, characterized in that: The cyclic monomer is one or more of ethylene oxide and propylene oxide, and the cyclic monomer in the dispersant is a mixture of ethylene oxide and propylene oxide in a molar ratio of 1 to 6:
1.
6. The method according to claim 2, characterized in that The initiator is one of ammonium persulfate, diisopropyl peroxydicarbonate and dihexyl peroxydicarbonate; the chain transfer agent is one of thioglycolic acid, mercaptoethanol and mercaptopropionic acid; and the ether substance is diethylene glycol monoallyl ether or propylene glycol monoallyl ether.
7. The method according to claim 2, characterized in that The amine head is N-methyl-allylamine; the reducing agent is sodium hypophosphite; the neutralizing agent is potassium carbonate; and the carboxyl head in the intercalating agent is tiglic acid.
8. The method according to claim 2, characterized in that: The alcohol-ether ratio is 1.7-2.5:
1.
9. The method according to claim 2, characterized in that: The molar ratio of the dispersant, the water retaining agent, the intercalating agent and the polymerized polyol is 2:1:1:
4.
10. The method according to claim 2, characterized in that The polymeric polyol is composed of several of ethylene glycol, glycerol, trimeryl glycol and triethanolamine.