Mortar additive and preparation process thereof

By optimizing the combination of water-reducing agents, thickeners, and water-retaining agents and controlling the adsorption rate, the problem of unstable adsorption of concrete mortar additives was solved, thus achieving stability of concrete performance and controllability of the construction process.

CN118930119APending Publication Date: 2024-11-12JIANGSU XIANSHUAI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411133823.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

If the adsorption rate of concrete mortar additives is too fast or too slow, it will lead to unstable concrete fluidity and early strength development, affecting construction operation time and performance.

Method used

By using a specific ratio of water-reducing agent, thickener, and water-retaining agent, and by adjusting the flexibility of the molecular chain and the distribution of adsorption groups, the polycarboxylate superplasticizer is gradually and uniformly adsorbed onto the surface of cement particles, thereby controlling the adsorption rate and optimizing the composition ratio of the polycarboxylate superplasticizer.

Benefits of technology

It stabilizes the adsorption rate of the water-reducing agent, ensuring the consistency of concrete performance and the controllability of the construction process, avoiding the problem of adsorption rate being too fast or too slow, and improving the fluidity and early strength of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930119A_ABST
    Figure CN118930119A_ABST
Patent Text Reader

Abstract

The mortar additive comprises a water reducing agent, a thickening agent and a water-retaining agent, and the water reducing agent is prepared from, by weight, 10-20 parts of methyl allyl polyoxyethylene ether, 8-14 parts of isobutenol polyoxyethylene ether, 2-6 parts of adipic acid, 10-15 parts of hydrogen peroxide, 5-12 parts of acrylic acid, 5-10 parts of sodium hydride, 5-10 parts of ferrous sulfate, 10-18 parts of VC and 60-65 parts of deionized water. According to the invention, the methylallyl polyoxyethylene ether and the isobutylene alcohol polyoxyethylene ether are uniformly distributed on a molecular chain, so that the water reducer can be gradually released and uniformly adsorbed on the surface of cement particles, thereby avoiding the problem of too high adsorption speed, and the adipic acid and the acrylic acid regulate the flexibility of the molecular chain and the distribution of adsorption groups. The adsorption process is more stable, the water reducing effect is ensured, the adsorption speed of the water reducing agent is stabilized, and the consistency of concrete performance and the controllability of the construction process are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of concrete admixtures, and in particular to a mortar additive and a preparation process thereof. Background Art

[0002] Mortar additives are chemical materials used to improve the performance of mortar. Their main function is to improve the strength, fluidity, water retention and crack resistance of mortar. Common mortar additives include water reducers, enhancers, thickeners, plasticizers and water retainers. Among them, concrete mortar with high strength and good durability has become the focus of research. Enhancers or water reducers that can increase the strength and durability of concrete mortar can be adsorbed on the surface of cement particles, reduce the interaction between particles, improve the fluidity and dispersibility of concrete, and improve the strength, durability and working performance of concrete.

[0003] However, the adsorption rate of concrete mortar is usually the rate at which mortar admixtures are adsorbed onto the surface of cement particles in cement paste. When the adsorption rate of additives in concrete mortar increases excessively, it is easy for the water reducer to lose its effectiveness in a short period of time, causing the fluidity of concrete to drop rapidly, thereby affecting plasticity retention and construction operation time. When the adsorption rate of additives in concrete mortar decreases excessively, the dispersion of cement particles will increase more slowly, resulting in insufficient development of early strength of concrete. Summary of the invention

[0004] The object of the present invention is to provide a mortar additive and a preparation process thereof to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a mortar additive, comprising a water reducing agent, a thickener and a water retaining agent, wherein the water reducing agent is composed of the following raw materials in parts by weight: 10-20 parts of methyl allyl polyoxyethylene ether, 8-14 parts of isobutylene alcohol polyoxyethylene ether, 2-6 parts of adipic acid, 10-15 parts of hydrogen peroxide, 5-12 parts of acrylic acid, 5-10 parts of sodium hydride, 5-10 parts of ferrous sulfate, 10-18 parts of VC and 60-65 parts of deionized water;

[0006] The thickener is composed of the following raw materials in parts by weight: 15-30 parts of sepiolite powder, 0.3-0.5 parts of ethyl cellulose, 80-120 parts of fly ash and 2-3 parts of sodium lignin sulfonate;

[0007] The water retaining agent is composed of the following raw materials in parts by weight: 4-6 parts of methacrylic acid, 6-10 parts of N-vinyl pyrrolidone, 1.5-2.5 parts of sodium methacryloyloxyethyl sulfonate and 1-3 parts of guar gum.

[0008] Preferably, the water reducer is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 3 parts of adipic acid, 10 parts of hydrogen peroxide, 6 parts of acrylic acid, 5 parts of sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC and 60 parts of deionized water.

[0009] Preferably, the water reducer is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 5 parts of adipic acid, 10 parts of hydrogen peroxide, 10 parts of acrylic acid, 5 parts of sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC and 60 parts of deionized water.

[0010] Preferably, the water reducer is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 4 parts of adipic acid, 10 parts of hydrogen peroxide, 8 parts of acrylic acid, sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC, and 60 parts of deionized water.

[0011] Preferably, the thickener is composed of the following raw materials in parts by weight: 25 parts of sepiolite powder, 0.5 parts of ethyl cellulose, 110 parts of fly ash and 3 parts of sodium lignin sulfonate.

[0012] Preferably, the thickener is composed of the following raw materials in parts by weight: 20 parts of sepiolite powder, 0.4 parts of ethyl cellulose, 90 parts of fly ash and 2 parts of sodium lignin sulfonate.

[0013] Preferably, the water retaining agent is composed of the following raw materials in parts by weight: 5 parts of methacrylic acid, 8 parts of N-vinyl pyrrolidone, 2 parts of sodium methacryloyloxyethyl sulfonate and 2 parts of guar gum.

[0014] The present invention also provides a preparation process of a mortar additive, comprising the following steps:

[0015] S1: Add methyl allyl polyoxyethylene ether solution into a reactor, stir at a uniform speed and add ammonium persulfate and hydrogen peroxide, mix isobutylene alcohol polyoxyethylene ether, adipic acid, acrylic acid and deionized water in proportion and stir to prepare material A, mix VC, sodium hydride and ferrous sulfate with an appropriate amount of deionized water in proportion and stir to prepare material B, gradually add material A and material B dropwise in the reactor to obtain a water reducer.

[0016] S2: Add methacrylic acid, N-vinyl pyrrolidone and sodium methacryloyloxyethyl sulfonate into the reactor, stir evenly to fully mix the monomers, add ammonium sulfate during the monomer mixing to carry out polymerization reaction, and add guar gum solution after 15 minutes of polymerization reaction, continue the reaction until completion, and obtain a water retaining agent.

[0017] S3: Mix sepiolite powder and fly ash in a ratio of 1:5 to obtain a dry mixture, add ethyl cellulose solution and sodium lignin sulfonate to the dry mixture, and continue stirring until all ingredients are evenly mixed to obtain a thickener.

[0018] S4: Put the water reducing agent into a mixing container and stir it evenly. During the stirring process, add the water retaining agent into the water reducing agent, and then gradually add the thickener. After mixing the water reducing agent, thickener and water retaining agent, continue stirring for 15-30 minutes. After there is no obvious lumps and all the ingredients are completely mixed, the prepared mortar additive is obtained.

[0019] Preferably, isobutylene alcohol polyoxyethylene ether, adipic acid, acrylic acid and deionized water are mixed in a ratio of 1:2:2:10.

[0020] Preferably, after material B is added dropwise for 3 hours, the solution is kept warm for 2 hours, and then the solution is neutralized with 20% sodium hydroxide to a pH of 6-7.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: the mortar additive provided by the present invention can be gradually released and uniformly adsorbed on the surface of cement particles, thereby avoiding the problem of too fast adsorption speed; adipic acid (AA) and acrylic acid (HEA) regulate the flexibility of the molecular chain and the distribution of the adsorption groups, making the adsorption process smoother, ensuring the water-reducing effect while stabilizing the adsorption speed of the water-reducing agent, thereby ensuring the consistency of concrete performance and the controllability of the construction process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a schematic diagram of the preparation process of the mortar additive according to the embodiment of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1

[0025] An embodiment of the present invention provides a mortar additive, which is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 3 parts of adipic acid, 10 parts of hydrogen peroxide, 6 parts of acrylic acid, 5 parts of sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC and 60 parts of deionized water.

[0026] The thickener is composed of the following raw materials in parts by weight: 15 parts of sepiolite powder, 0.3 parts of ethyl cellulose, 80 parts of fly ash and 2 parts of sodium lignin sulfonate.

[0027] The water retaining agent is composed of the following raw materials in parts by weight: 4 parts of methacrylic acid, 6 parts of N-vinyl pyrrolidone, 1.5 parts of sodium methacryloyloxyethyl sulfonate and 1 part of guar gum.

[0028] Embodiment 2

[0029] An embodiment of the present invention provides a mortar additive, which is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 5 parts of adipic acid, 10 parts of hydrogen peroxide, 10 parts of acrylic acid, 5 parts of sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC and 60 parts of deionized water.

[0030] The thickener is composed of the following raw materials in parts by weight: 15 parts of sepiolite powder, 0.3 parts of ethyl cellulose, 80 parts of fly ash and 2 parts of sodium lignin sulfonate.

[0031] The water retaining agent is composed of the following raw materials in parts by weight: 4 parts of methacrylic acid, 6 parts of N-vinyl pyrrolidone, 1.5 parts of sodium methacryloyloxyethyl sulfonate and 1 part of guar gum.

[0032] Embodiment 3

[0033] An embodiment of the present invention provides a mortar additive, which is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 4 parts of adipic acid, 10 parts of hydrogen peroxide, 8 parts of acrylic acid, sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC, and 60 parts of deionized water.

[0034] The thickener is composed of the following raw materials in parts by weight: 20 parts of sepiolite powder, 0.4 parts of ethyl cellulose, 90 parts of fly ash and 2 parts of sodium lignin sulfonate.

[0035] The water retaining agent is composed of the following raw materials in parts by weight: 5 parts of methacrylic acid, 8 parts of N-vinyl pyrrolidone, 2 parts of sodium methacryloyloxyethyl sulfonate and 2 parts of guar gum.

[0036] Embodiment 4

[0037] An embodiment of the present invention provides a mortar additive, which is composed of the following raw materials in parts by weight: 18 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 4 parts of adipic acid, 10 parts of hydrogen peroxide, 8 parts of acrylic acid, sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC, and 60 parts of deionized water.

[0038] The thickener is composed of the following raw materials in parts by weight: 20 parts of sepiolite powder, 0.4 parts of ethyl cellulose, 90 parts of fly ash and 2 parts of sodium lignin sulfonate.

[0039] The water retaining agent is composed of the following raw materials in parts by weight: 5 parts of methacrylic acid, 8 parts of N-vinyl pyrrolidone, 2 parts of sodium methacryloyloxyethyl sulfonate and 2 parts of guar gum.

[0040] See also Figure 1 , an embodiment of the present invention provides a preparation process of a mortar additive, comprising the following steps:

[0041] S1: Add methyl allyl polyoxyethylene ether solution into a reactor, stir at a uniform speed and add ammonium persulfate and hydrogen peroxide, mix isobutylene alcohol polyoxyethylene ether, adipic acid, acrylic acid and deionized water in proportion and stir to prepare material A, mix VC, sodium hydride and ferrous sulfate with an appropriate amount of deionized water in proportion and stir to prepare material B, gradually add material A and material B dropwise in the reactor to obtain a water reducer.

[0042] S2: Add methacrylic acid, N-vinyl pyrrolidone and sodium methacryloyloxyethyl sulfonate into the reactor, stir evenly to fully mix the monomers, add ammonium sulfate during the monomer mixing to carry out polymerization reaction, and add guar gum solution after 15 minutes of polymerization reaction, continue the reaction until completion, and obtain a water retaining agent.

[0043] S3: Mix sepiolite powder and fly ash in a ratio of 1:5 to obtain a dry mixture, add ethyl cellulose solution and sodium lignin sulfonate to the dry mixture, and continue stirring until all ingredients are evenly mixed to obtain a thickener.

[0044] S4: Put the water reducing agent into a mixing container and stir it evenly. During the stirring process, add the water retaining agent into the water reducing agent, and then gradually add the thickener. After mixing the water reducing agent, thickener and water retaining agent, continue stirring for 15-30 minutes. After there is no obvious lumps and all the ingredients are completely mixed, the prepared mortar additive is obtained.

[0045] Among them, after material B was added dropwise for 3 hours, the solution was kept warm for 2 hours, and then 20% sodium hydroxide was used to neutralize the solution to a pH of 6-7.

[0046] The mortar additive raw materials provided in Examples 1 to 4 are weighed, and the weighed mortar additive raw materials are used to prepare the mortar additive according to the above-mentioned mortar additive preparation process.

[0047] Among them, the isothermal adsorption test is carried out by sampling the mortar additives of Examples 1 to 4 prepared by the preparation process of the mortar additive and filtering them, and mixing the four filtrates with the mortar samples under constant temperature conditions for 12 hours. After the mixing reaction, the mortar particles are removed by filter paper to obtain a clear liquid, and the additive concentration in the filtrate is determined by spectrophotometry, and the adsorption amount of the additive is calculated based on the difference between the initial mortar additive concentration and the concentration in the filtrate.

[0048] Table 1 shows the test results of mortar additives:

[0049]

[0050] In summary: It can be seen from Table 1 that after the mortar additive provided in Example 3 was tested for adsorption in three time periods, the results showed that the adsorption amount of the mortar additive changed more steadily, and there was no significant increase or decrease in the adsorption amount, thereby ensuring the adsorption rate of the mortar additive within a certain period of time.

[0051] The invention can effectively stabilize the adsorption speed of the water reducer by optimizing the component ratio of the polycarboxylate water reducer, wherein the uniform distribution of methyl allyl polyoxyethylene ether (TPEG) and isobutylene alcohol polyoxyethylene ether (HPEG) on the molecular chain enables the water reducer to be gradually released and uniformly adsorbed on the surface of cement particles, thereby avoiding the phenomenon of too fast adsorption speed, adipic acid (AA) and acrylic acid (HEA) further regulate the flexibility of the molecular chain and the distribution of adsorption groups, making the adsorption process more stable, and finally by adjusting the pH value of the solution, the water reducer can stabilize the adsorption speed while ensuring the water reduction effect, thereby ensuring the consistency of concrete performance and the controllability of the construction process.

[0052] Parts not involved in the present invention are the same as the prior art or can be implemented by the prior art. Although the embodiments of the present invention have been shown and described, it is understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A mortar additive, comprising a water reducing agent, a thickener and a water retaining agent, characterized in that: The water reducer is composed of the following raw materials in parts by weight: 10-20 parts of methyl allyl polyoxyethylene ether, 8-14 parts of isobutylene alcohol polyoxyethylene ether, 2-6 parts of adipic acid, 10-15 parts of hydrogen peroxide, 5-12 parts of acrylic acid, 5-10 parts of sodium hydride, 5-10 parts of ferrous sulfate, 10-18 parts of VC and 60-65 parts of deionized water; The thickener is composed of the following raw materials in parts by weight: 15-30 parts of sepiolite powder, 0.3-0.5 parts of ethyl cellulose, 80-120 parts of fly ash and 2-3 parts of sodium lignin sulfonate; The water retaining agent is composed of the following raw materials in parts by weight: 4-6 parts of methacrylic acid, 6-10 parts of N-vinyl pyrrolidone, 1.5-2.5 parts of sodium methacryloyloxyethyl sulfonate and 1-3 parts of guar gum.

2. A mortar additive according to claim 1, characterized in that: The water reducer is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 3 parts of adipic acid, 10 parts of hydrogen peroxide, 6 parts of acrylic acid, 5 parts of sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC and 60 parts of deionized water.

3. A mortar additive according to claim 1, characterized in that: The water reducer is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 5 parts of adipic acid, 10 parts of hydrogen peroxide, 10 parts of acrylic acid, 5 parts of sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC and 60 parts of deionized water.

4. A mortar additive according to claim 1, characterized in that: The water reducer is composed of the following raw materials in parts by weight: 15 parts of methyl allyl polyoxyethylene ether, 10 parts of isobutylene alcohol polyoxyethylene ether, 4 parts of adipic acid, 10 parts of hydrogen peroxide, 8 parts of acrylic acid, sodium hydride, 7 parts of ferrous sulfate, 12 parts of VC, and 60 parts of deionized water.

5. The mortar additive according to claim 1, characterized in that: The thickener is composed of the following raw materials in parts by weight: 25 parts of sepiolite powder, 0.5 parts of ethyl cellulose, 110 parts of fly ash and 3 parts of sodium lignin sulfonate.

6. A mortar additive according to claim 1, characterized in that: The thickener is composed of the following raw materials in parts by weight: 20 parts of sepiolite powder, 0.4 parts of ethyl cellulose, 90 parts of fly ash and 2 parts of sodium lignin sulfonate.

7. A mortar additive according to claim 1, characterized in that: The water retaining agent is composed of the following raw materials in parts by weight: 5 parts of methacrylic acid, 8 parts of N-vinyl pyrrolidone, 2 parts of sodium methacryloyloxyethyl sulfonate and 2 parts of guar gum.

8. The preparation process of a mortar additive according to claim 1, characterized in that: The following steps are involved: S1: Add methyl allyl polyoxyethylene ether solution into a reactor, stir at a uniform speed and add ammonium persulfate and hydrogen peroxide, mix isobutylene alcohol polyoxyethylene ether, adipic acid, acrylic acid and deionized water in proportion and stir to prepare material A, mix VC, sodium hydride and ferrous sulfate with an appropriate amount of deionized water in proportion and stir to prepare material B, gradually add material A and material B dropwise in the reactor to obtain a water reducer. S2: Add methacrylic acid, N-vinyl pyrrolidone and sodium methacryloyloxyethyl sulfonate into the reactor, stir evenly to fully mix the monomers, add ammonium sulfate during the monomer mixing to carry out polymerization reaction, and add guar gum solution after 15 minutes of polymerization reaction, continue the reaction until completion, and obtain a water retaining agent. S3: Mix sepiolite powder and fly ash in a ratio of 1:5 to obtain a dry mixture, add ethyl cellulose solution and sodium lignin sulfonate to the dry mixture, and continue stirring until all ingredients are evenly mixed to obtain a thickener. S4: Put the water reducing agent into a mixing container and stir it evenly. During the stirring process, add the water retaining agent into the water reducing agent, and then gradually add the thickener. After mixing the water reducing agent, thickener and water retaining agent, continue stirring for 15-30 minutes. After there is no obvious lumps and all the ingredients are completely mixed, the prepared mortar additive is obtained.

9. The preparation process of a mortar additive according to claim 8, characterized in that: In S2, isobutylene alcohol polyoxyethylene ether, adipic acid, acrylic acid and deionized water are mixed in a ratio of 1:2:2: