Acid-base modified corrosion-resistant coal gasification slag filling material and preparation method thereof

The gasification slag is treated through acid-base modification and nanocomposite emulsion, and combined with alkali exciters to promote gel generation, the problems of gasification slag stacking and mine water corrosion are solved, and the corrosion resistance and resource utilization efficiency of the filling materials are improved. It has achieved efficient treatment of coal-based solid waste and improved corrosion resistance of filling materials.

CN118930142AInactive Publication Date: 2024-11-12CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202411010318.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The gasified slag generated in coal mining occupies land and pollutes the environment. The mine water corrodes the filling materials, reducing its mechanical properties. It is difficult for the existing technology to effectively dispose of and improve its corrosion resistance.

Method used

Through acid-base modification, the coal gasification slag is strengthened, and nanocomposite emulsions and alkali excitants are added to promote the generation of Na and K gels, enhance the permeability and water resistance of the filling materials, and form acid-base modified corrosion-resistant coal gasification slag filling materials. .

Benefits of technology

It significantly improves the mineral water corrosion resistance of coal gasified slag filling materials, realizes the resource utilization of coal-based solid waste and the corrosion resistance of filling materials, and is economical in technology and green in environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an acid-base modified corrosion-resistant coal gasification slag filling material and a preparation method thereof, and belongs to the field of solid waste resource utilization and filling materials. The filling material comprises the following components in parts by weight: 5-20 parts of coal gasification slag powder, 2-10 parts of slag, 20-50 parts of coal gasification slag coarse aggregate, 0.1-0.5 part of an acidic molecule modifier, 0.1-1.5 parts of a nano composite emulsion, 0.5-5 parts of an alkaline activator and 16-45 parts of water. The preparation method comprises the following steps: firstly, uniformly mixing and stirring coal gasification slag powder and an acidic molecule modifier, carrying out ball milling in a ball mill, and standing to obtain first mixed powder; then mixing and stirring the first mixed powder and slag, adding a nano composite emulsion, and carrying out ball milling in a ball mill to obtain a second mixed material; and then sequentially adding the alkali activator, water and the coal gasification slag coarse aggregate, and mixing and stirring to obtain the filling material. The prepared acid-base modified filling material has the advantages of being high in mine water corrosion resistance, low in cost, excellent in performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solid waste resource utilization and filling materials, and specifically relates to an acid-base modified corrosion-resistant coal gasification slag filling material and a preparation method thereof. Background Art

[0002] There are two main types of technical problems commonly encountered in coal mining: coal-based solid waste pollution and mine water risks, which are as follows.

[0003] First of all, a large amount of coal gasification slag will be produced during the gasification process. The stacking of coal gasification slag not only occupies a large amount of land, but also causes serious pollution to the environment. Making the coal gasification slag into filling materials and transporting it to the underground space can achieve the dual functions of resource utilization of coal-based solid waste and controlling surface subsidence.

[0004] Secondly, a large amount of mine water is also produced during coal mining. Mine water is generally acidic, with a pH value of 2-8, which will corrode the filling material and reduce its mechanical properties.

[0005] However, for the backfill mining industry, how to improve the disposal of coal gasification slag and enhance the corrosion resistance of backfill materials to mine water are the main problems currently faced.

[0006] Therefore, the present invention proposes to enhance the activity of coal gasification slag by acid-base modification, and add nano-composite emulsion to enhance the permeability and water resistance of coal gasification slag filling materials. In addition, alkaline activators are added to promote the formation of Na and K gels, in order to provide a new mine water corrosion-resistant material for coal-based solid waste utilization and filling mining. Summary of the invention

[0007] Purpose of the invention: In view of the deficiencies in the prior art, the present invention provides an acid-base modified corrosion-resistant coal gasification slag filling material and a preparation method thereof, wherein the activity of the coal gasification slag is enhanced by acid modification, and a nano-composite emulsion is added to enhance the permeability and water resistance of the coal gasification slag filling material, and an alkali activator is added to promote the formation of Na and K gels, so as to achieve the purpose of improving the corrosion resistance of the coal gasification slag filling material.

[0008] Technical solution: To achieve the above purpose, the technical solution adopted by the present invention is:

[0009] The first object of the present invention is to provide an acid-base modified corrosion-resistant coal gasification slag filling material. The composition of the mine water corrosion-resistant coal-based solid waste filling paste formed by the acid-base modified corrosion-resistant coal gasification slag filling material includes, by weight: 5-20 parts of coal gasification slag powder, 2-10 parts of slag, 20-50 parts of coal gasification slag coarse aggregate, 0.1-0.5 parts of acidic molecular modifier, 0.1-1.5 parts of nano-composite emulsion, 0.5-5 parts of alkaline activator, and 16-45 parts of water, wherein the nano-composite emulsion includes at least one of styrene acrylic emulsion, alcohol ester twelve, and polyurethane.

[0010] Optionally, the composition of the acid-base modified corrosion-resistant coal gasification slag filling material is calculated in percentage by weight.

[0011] Optionally, the acidic molecular modifier includes at least one of salicylic acid, tartaric acid and malic acid. The acidic molecular modifier can react with the oxides in the coal gasification slag to increase its specific surface area and hydration activity.

[0012] Further optionally, the acidic molecular modifier is a mixture of salicylic acid, tartaric acid and malic acid.

[0013] Further optionally, the acidic molecular modifier is a mixture of salicylic acid, tartaric acid, and malic acid in a weight ratio of (30-60): (15-25): (5-55).

[0014] Optionally, the nanocomposite emulsion has the characteristics of high molecular weight and fast polymerization rate, and can penetrate into the microscopic pores of the filling material, fill small cracks and gaps, and at the same time form a nanoscale network structure inside the material to enhance the permeability and water resistance of the filling material.

[0015] Further optionally, the nanocomposite emulsion is a mixture of styrene acrylic emulsion, alcohol ester dodecaned and polyurethane.

[0016] Further optionally, the nanocomposite emulsion comprises, by weight: 30-70 parts of styrene acrylic emulsion, 20-50 parts of alcohol ester dodecanedione, and 5-20 parts of polyurethane.

[0017] Optionally, the alkaline activator includes at least one of sodium hydroxide, potassium hydroxide, and sodium silicate. Adding a certain amount of alkaline activator helps to promote the formation of Na and K gels, which is beneficial to stimulating the hydration activity of the material. In addition, sodium hydroxide, potassium hydroxide, and sodium silicate are all common low-cost alkaline substances that are easily available.

[0018] Further optionally, the alkaline activator is a mixture of sodium hydroxide, potassium hydroxide and sodium silicate.

[0019] Further optionally, the alkaline activator comprises, by weight: 20-60 parts of sodium hydroxide, 5-20 parts of potassium hydroxide, and 20-85 parts of sodium silicate.

[0020] Further optionally, the sodium silicate is sodium silicate having a water glass modulus of 2.5-3.5.

[0021] Optionally, the particle size of the coal gasification slag powder is not greater than 200 μm.

[0022] Further optionally, the particle size of the coal gasification slag powder is not higher than 100 μm.

[0023] Optionally, the particle size of the coal gasification slag coarse aggregate is not higher than 30 mm.

[0024] Further optionally, the particle size of the coal gasification slag coarse aggregate is 15-30 mm.

[0025] The second object of the present invention is to provide a method for preparing an acid-base modified corrosion-resistant coal gasification slag filling material, comprising the following steps:

[0026] S1. Mix the coal gasification slag powder and the acidic molecular modifier and stir them evenly, and put them into a ball mill to obtain a first mixed powder; ball milling helps to modify the acidic molecules and activate the coal gasification slag powder;

[0027] S2, mixing the first mixed powder with slag, adding nanocomposite emulsion, and grinding in a ball mill to obtain a second mixed material; ball milling modification to increase its hydration activity;

[0028] S3. Add alkali activator, water and coal gasification slag coarse aggregate into the second mixture, mix and stir to obtain filling material.

[0029] Optionally, in step S1, the ball milling time is 15-45 minutes.

[0030] Optionally, in step S1, the rotation speed of the ball mill is 520 r / min.

[0031] Optionally, in step S2, the first mixed powder is mixed with slag and stirred for 3-5 minutes.

[0032] Optionally, in step S2, a nanocomposite emulsion is added and the mixture is placed in a ball mill for 15-40 minutes.

[0033] Optionally, in step S2, the rotation speed of the ball mill is 400 r / min.

[0034] Optionally, in step S3, the order of adding the alkali activator, water, and coal gasification slag coarse aggregate is to add the alkali activator, water, and coal gasification slag coarse aggregate in sequence.

[0035] Optionally, in step S3, the alkali activator, water, and coal gasification slag coarse aggregate are added and mixed and stirred for 5-10 minutes.

[0036] Optionally, the method for preparing the acid-base modified corrosion-resistant coal gasification slag filling material comprises the following steps:

[0037] S1. Mix the coal gasification slag powder and the acidic molecular modifier and stir them evenly, put them into a ball mill and mill them for 15-45 minutes to obtain a first mixed powder;

[0038] S2, mixing the first mixed powder after ball milling with slag for 3-5 minutes, adding the nanocomposite emulsion, and putting it into a ball mill for 15-40 minutes to obtain a second mixed material;

[0039] S3. Add alkali activator, water and coal gasification slag coarse aggregate to the second mixture in sequence, mix and stir to obtain filling material.

[0040] Optionally, the components are measured by weight, and the preparation method of the acid-base modified corrosion-resistant coal gasification slag filling material comprises the following steps:

[0041] S1. Mix 5-10 parts of coal gasification slag powder and 0.1-0.5 parts of acidic molecular modifier, stir evenly, put them into a ball mill for 15-45 minutes, and obtain the first mixed powder; this step modifies the coal gasification slag powder, increases its specific surface area, and increases its hydration activity.

[0042] S2, mixing the first mixed powder after ball milling with slag for 3-5 minutes, adding nano-composite emulsion, and putting it into a ball mill for 15-40 minutes to obtain a second mixed material; this step modifies the powder used, reduces the particle size, and increases the hydration activity.

[0043] S3. Add alkali activator, water and coal gasification slag coarse aggregate to the second mixture in sequence, mix and stir to obtain filling material.

[0044] The third object of the present invention is to provide an application of the above method or coal gasification slag filling material resistant to mine water corrosion in the field of coal gasification slag filling.

[0045] Beneficial effects: The acid-base modified corrosion-resistant coal gasification slag filling material and its preparation method provided by the present invention have the following advantages compared with the existing filling materials and preparation methods:

[0046] (1) Using the combined preparation process of acid modification-organic-inorganic nanocomposite emulsion-alkali modification to activate coal gasification slag and comprehensively improve corrosion resistance;

[0047] (2) Acid modification strengthens the activity of coal gasification slag, nanocomposite emulsion enhances the permeability and water resistance of coal gasification slag filling materials, and the addition of alkaline activator promotes the formation of Na and K gels;

[0048] (3) Realize large-scale utilization of coal gasification slag, which is economical, green and environmentally friendly; and significantly improve the mine water corrosion resistance of coal gasification slag filling materials. DETAILED DESCRIPTION

[0049] The purpose of the present invention is to provide an acid-base modified corrosion-resistant coal gasification slag filling material and a preparation method thereof, aiming to enhance the activity of coal gasification slag, improve the strength of the filling material, increase the corrosion resistance of the filling material, and realize large-scale disposal and utilization of coal gasification ash.

[0050] The present invention relates to an acid-base modified corrosion-resistant coal gasification slag filling material and a preparation method thereof, and belongs to the field of solid waste resource utilization and filling materials. The acid-base modified corrosion-resistant coal gasification slag filling material of the present invention is composed of 5-20 parts of coal gasification slag powder, 2-10 parts of slag, 20-50 parts of coal gasification slag coarse aggregate, 0.1-0.5 parts of acidic molecular modifier, 0.1-1.5 parts of nano-composite emulsion, 0.5-5 parts of alkaline activator, and 16-45 parts of water, wherein the nano-composite emulsion includes at least one of styrene-acrylic emulsion, alcohol ester twelve, and polyurethane.

[0051] The preparation method of the acid-base modified corrosion-resistant coal gasification slag filling material of the present invention comprises the following steps:

[0052] S1. Mix 5-10 parts of coal gasification slag powder and 0.1-0.5 parts of acidic molecular modifier, stir evenly, put them into a ball mill and mill for 15-45 minutes to obtain a first mixed powder;

[0053] S2, mixing the first mixed powder after ball milling with slag for 3-5 minutes, adding the nanocomposite emulsion, and putting it into a ball mill for 15-40 minutes to obtain a second mixed material;

[0054] S3. Add alkali activator, water and coal gasification slag coarse aggregate to the second mixture in sequence, mix and stir for 5-10 minutes to obtain filling material.

[0055] The present invention will be further described below in conjunction with examples. According to the following examples, the present invention can be better understood. However, it is easy for those skilled in the art to understand that the specific material ratios, process conditions and results described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.

[0056] Comparative Example 1

[0057] In this comparative example, no acidic molecular modifier was added, and the purpose was to study the effect of the acidic molecular modifier on the filling material.

[0058] S1. Weigh 5 parts of coal gasification slag powder (particle size less than 100 μm) and put it into a ball mill for 15 minutes at a speed of 520 r / min to obtain a first mixed powder;

[0059] S2, then the first mixed powder and 2 parts of slag were mixed and stirred for 3 minutes, 0.1 parts of nanocomposite emulsion (30 parts of styrene acrylic emulsion, 20 parts of alcohol ester twelve, 5 parts of polyurethane) were added, and the mixture was put into a ball mill and ball-milled at a rate of 400r / min for 15 minutes to obtain a second mixed material;

[0060] S3. Add 20 parts of gasification slag coarse aggregate (particle size is 15-20mm), 0.5 parts of alkali activator (40 parts of sodium hydroxide, 15 parts of potassium hydroxide, 55 parts of sodium silicate with a water glass modulus of 3) and 16 parts of water to the second mixture in sequence, mix and stir for 5 minutes to obtain the filling material.

[0061] Then pour the filling material into the triple mold with silicone oil brushed inside, put it on the vibrator and shake it for 30 seconds. After 24 hours, demould it and put it in a curing box with a temperature of 20°C and a humidity of 95%. Cured it for 28 days to obtain the test piece.

[0062] Soak part of the filling paste in a corrosion solution with a pH of 4, a chloride ion concentration of 3%, and a sulfate ion concentration of 6% for 12 hours, then take it out, dry the surface moisture with absorbent paper, and bake it in an oven at a temperature of 35°C for 12 hours. Repeat this step 12 times. Test the uniaxial compressive strength of the curing material before and after corrosion.

[0063] A layer of melted paraffin with a small amount of rosin is coated on the sides of another part of the specimens, and then the specimens are pressed into the test mold with a pressurizer. The water seepage height of the specimens is tested using a fully automatic water penetration tester with a set water pressure of 1.2MPa and a pressurization time of 24h.

[0064] Comparative Example 2

[0065] In this comparative example, no alkali activator was added, and the purpose was to study the effect of the alkali activator on the filling material.

[0066] S1, weigh 5 parts of coal gasification slag powder (particle size less than 100 μm) and 0.1 parts of acidic molecular modifier (50 parts of salicylic acid, 20 parts of tartaric acid, 35 parts of malic acid), mix them evenly, put them into a ball mill and mill them at a speed of 520 r / min for 15 minutes to obtain a first mixed powder;

[0067] S2, then the first mixed powder and 2 parts of slag were mixed and stirred for 3 minutes, 0.1 parts of nanocomposite emulsion (30 parts of styrene acrylic emulsion, 20 parts of alcohol ester twelve, 5 parts of polyurethane) were added, and the mixture was put into a ball mill and ball-milled at a rate of 400r / min for 15 minutes to obtain a second mixed material;

[0068] S3. Add 20 parts of coal gasification slag coarse aggregate (particle size is 15-20 mm) and 16 parts of water to the second mixture in sequence, mix and stir for 5 minutes to obtain filling material.

[0069] Then pour the filling material into the triple mold with silicone oil brushed inside, put it on the vibrator and shake it for 30 seconds. After 24 hours, demould it and put it in a curing box with a temperature of 20°C and a humidity of 95%. Cured it for 28 days to obtain the test piece.

[0070] Soak part of the filling paste in a corrosion solution with a pH of 4, a chloride ion concentration of 3%, and a sulfate ion concentration of 6% for 12 hours, then take it out, dry the surface moisture with absorbent paper, and bake it in an oven at a temperature of 35°C for 12 hours. Repeat this step 12 times. Test the uniaxial compressive strength of the curing material before and after corrosion.

[0071] A layer of melted paraffin with a small amount of rosin is coated on the sides of another part of the specimens, and then the specimens are pressed into the test mold with a pressurizer. The water seepage height of the specimens is tested using a fully automatic water penetration tester with a set water pressure of 1.2MPa and a pressurization time of 24h.

[0072] Comparative Example 3

[0073] In this comparative example, no nanocomposite emulsion was added, and the purpose was to study the effect of the nanocomposite emulsion on the filling material.

[0074] S1, weigh 5 parts of coal gasification slag powder (particle size less than 100 μm) and 0.1 parts of acidic molecular modifier (50 parts of salicylic acid, 20 parts of tartaric acid, 35 parts of malic acid), mix them evenly, put them into a ball mill and mill them at a speed of 520 r / min for 15 minutes to obtain a first mixed powder;

[0075] S2, then mixing the first mixed powder with 2 parts of slag for 3 minutes, putting it into a ball mill and ball milling it at a rate of 400 r / min for 15 minutes to obtain a second mixed material;

[0076] S3. Add 20 parts of gasification slag coarse aggregate (particle size is 15-20mm), 0.5 parts of alkali activator (40 parts of sodium hydroxide, 15 parts of potassium hydroxide, 55 parts of sodium silicate with water glass modulus of 3) and 16 parts of water to the second mixture in sequence, mix and stir for 5 minutes to obtain filling material.

[0077] Then pour the filling material into the triple mold with silicone oil brushed inside, put it on the vibrator and shake it for 30 seconds. After 24 hours, demould it and put it in a curing box with a temperature of 20°C and a humidity of 95%. Cured it for 28 days to obtain the test piece.

[0078] Soak part of the filling paste in a corrosion solution with a pH of 4, a chloride ion concentration of 3%, and a sulfate ion concentration of 6% for 12 hours, then take it out, dry the surface moisture with absorbent paper, and bake it in an oven at a temperature of 35°C for 12 hours. Repeat this step 12 times. Test the uniaxial compressive strength of the curing material before and after corrosion.

[0079] A layer of melted paraffin with a small amount of rosin is coated on the sides of another part of the specimens, and then the specimens are pressed into the test mold with a pressurizer. The water seepage height of the specimens is tested using a fully automatic water penetration tester with a set water pressure of 1.2MPa and a pressurization time of 24h.

[0080] Example 1

[0081] S1, weigh 5 parts of coal gasification slag powder (particle size less than 100 μm) and 0.1 parts of acidic molecular modifier (50 parts of salicylic acid, 20 parts of tartaric acid, 35 parts of malic acid), mix them evenly, put them into a ball mill and mill them at a speed of 520 r / min for 15 minutes to obtain a first mixed powder;

[0082] S2, then the first mixed powder and 2 parts of slag were mixed and stirred for 3 minutes, 0.1 parts of nanocomposite emulsion (30 parts of styrene acrylic emulsion, 20 parts of alcohol ester twelve, 5 parts of polyurethane) were added, and the mixture was put into a ball mill and ball-milled for 15 minutes to obtain a second mixed material;

[0083] S3. Add 20 parts of gasification slag coarse aggregate (particle size is 15-20mm), 0.5 parts of alkali activator (40 parts of sodium hydroxide, 15 parts of potassium hydroxide, 55 parts of sodium silicate with a water glass modulus of 3) and 16 parts of water to the second mixture in sequence, mix and stir for 5 minutes to obtain the filling material.

[0084] Then pour the filling material into the triple mold with silicone oil brushed inside, put it on the vibrator and shake it for 30 seconds. After 24 hours, demould it and put it in a curing box with a temperature of 20°C and a humidity of 95%. Cured it for 28 days to obtain the test piece.

[0085] Soak part of the filling paste in a corrosion solution with a pH of 4, a chloride ion concentration of 3%, and a sulfate ion concentration of 6% for 12 hours, then take it out, dry the surface moisture with absorbent paper, and bake it in an oven at a temperature of 35°C for 12 hours. Repeat this step 12 times. Test the uniaxial compressive strength of the curing material before and after corrosion.

[0086] A layer of melted paraffin with a small amount of rosin is coated on the sides of another part of the specimens, and then the specimens are pressed into the test mold with a pressurizer. The water seepage height of the specimens is tested using a fully automatic water penetration tester with a set water pressure of 1.2MPa and a pressurization time of 24h.

[0087] Example 2

[0088] S1, weigh 10 parts of coal gasification slag powder (particle size less than 100 μm) and 0.3 parts of acidic molecular modifier (50 parts of salicylic acid, 20 parts of tartaric acid, 35 parts of malic acid), mix them evenly, put them into a ball mill and mill them at a speed of 520 r / min for 30 minutes to obtain a first mixed powder;

[0089] S2, then the first mixed powder and 5 parts of slag were mixed and stirred for 4 minutes, 1 part of nano-composite emulsion (30 parts of styrene-acrylic emulsion, 20 parts of alcohol ester twelve, 5 parts of polyurethane) was added, and the mixture was put into a ball mill and ball-milled for 25 minutes to obtain a second mixed material;

[0090] S3. Add 35 parts of gasification slag coarse aggregate (particle size is 15-20mm), 2.5 parts of alkali activator (40 parts of sodium hydroxide, 15 parts of potassium hydroxide, 55 parts of sodium silicate with water glass modulus of 3) and 25 parts of water to the second mixture in sequence, mix and stir for 8 minutes to obtain filling material.

[0091] Then pour the filling material into the triple mold with silicone oil brushed inside, put it on the vibrator and shake it for 30 seconds. After 24 hours, demould it and put it in a curing box with a temperature of 20°C and a humidity of 95%. Cured it for 28 days to obtain the test piece.

[0092] Soak part of the filling paste in a corrosion solution with a pH of 4, a chloride ion concentration of 3%, and a sulfate ion concentration of 6% for 12 hours, then take it out, dry the surface moisture with absorbent paper, and bake it in an oven at a temperature of 35°C for 12 hours. Repeat this step 12 times. Test the uniaxial compressive strength of the curing material before and after corrosion.

[0093] A layer of melted paraffin with a small amount of rosin is coated on the sides of another part of the specimens, and then the specimens are pressed into the test mold with a pressurizer. The water seepage height of the specimens is tested using a fully automatic water penetration tester with a set water pressure of 1.2MPa and a pressurization time of 24h.

[0094] Example 3

[0095] S1, weigh 20 parts of coal gasification slag powder (particle size less than 100 μm) and 0.5 parts of acidic molecular modifier (50 parts of salicylic acid, 20 parts of tartaric acid, 35 parts of malic acid), mix them evenly, put them into a ball mill and mill them at a speed of 520 r / min for 45 minutes to obtain a first mixed powder;

[0096] S2, then the first mixed powder and 10 parts of slag are mixed and stirred for 5 minutes, 1.5 parts of nanocomposite emulsion (30 parts of styrene acrylic emulsion, 20 parts of alcohol ester twelve, 5 parts of polyurethane) are added, and the mixture is put into a ball mill and ball milled at a rate of 400r / min for 40 minutes to obtain a second mixed material;

[0097] S3. Add 50 parts of coal gasification slag coarse aggregate (particle size is 15-20mm), 5 parts of alkali activator (40 parts of sodium hydroxide, 15 parts of potassium hydroxide, 55 parts of sodium silicate with a water glass modulus of 3) and 45 parts of water to the second mixture in sequence, mix and stir for 10 minutes to obtain the filling material.

[0098] Then pour the filling material into the triple mold with silicone oil brushed inside, put it on the vibrator and shake it for 30 seconds. After 24 hours, demould it and put it in a curing box with a temperature of 20°C and a humidity of 95%. Cured it for 28 days to obtain the test piece.

[0099] Soak part of the filling paste in a corrosion solution with a pH of 4, a chloride ion concentration of 3%, and a sulfate ion concentration of 6% for 12 hours, then take it out, dry the surface moisture with absorbent paper, and bake it in an oven at a temperature of 35°C for 12 hours. Repeat this step 12 times. Test the uniaxial compressive strength of the curing material before and after corrosion.

[0100] A layer of melted paraffin with a small amount of rosin is coated on the sides of another part of the specimens, and then the specimens are pressed into the test mold with a pressurizer. The water seepage height of the specimens is tested using a fully automatic water penetration tester with a set water pressure of 1.2MPa and a pressurization time of 24h.

[0101] Test Case

[0102] The corrosion-resistant coal gasification slag filling materials obtained in various embodiments and comparative examples were subjected to uniaxial compressive strength tests and water seepage height tests before and after corrosion. The results are shown in Table 1.

[0103] Table 1 Experimental results

[0104]

[0105]

[0106] From the above results, it can be found that compared with Example 1 in which the coal gasification slag powder is not treated with an acidic molecular modifier and Example 2 in which no alkaline activator is added, the uniaxial compressive strength of the filling material before and after corrosion is significantly improved in Examples 1-3 after the acidic molecular modifier and the alkaline activator are used, indicating that the strength of the filling material is significantly higher than that of Examples 1 and 2, indicating that the acidic molecular modifier can react with the substances in the coal gasification slag, increase its hydration activity, and thereby improve the mechanical properties of the filling material; the alkaline activator helps to promote the formation of gel, stimulate the hydration activity of the filling material, and improve the mechanical properties of the filling material.

[0107] Compared with the comparative example 3 without adding the nanocomposite emulsion, after adding the nanocomposite emulsion in the examples 1-3, the compressive strength of the filling materials after corrosion was lower than that of the uncorroded group, the corrosion resistance was greatly improved, and the water seepage height was also reduced.

[0108] The above results indicate that the acid-base modified corrosion-resistant coal gasification slag filling material of the present invention has excellent mechanical properties and water resistance, which effectively solves the problem of reduced corrosion strength of filling materials caused by mine water in the filling mining industry, and provides a new material for coal-based solid waste utilization and mine water corrosion resistance.

[0109] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An acid-base modified corrosion-resistant coal gasification slag filling material, characterized in that: The invention comprises, by weight, 5-20 parts of coal gasification slag powder, 2-10 parts of slag, 20-50 parts of coal gasification slag coarse aggregate, 0.1-0.5 parts of acidic molecular modifier, 0.1-1.5 parts of nano-composite emulsion, 0.5-5 parts of alkaline activator and 16-45 parts of water, wherein the nano-composite emulsion comprises at least one of styrene acrylic emulsion, alcohol ester dodecahydrate and polyurethane.

2. The acid-base modified corrosion-resistant coal gasification slag filling material according to claim 1, characterized in that: The acidic molecular modifier includes at least one of salicylic acid, tartaric acid and malic acid; preferably, the acidic molecular modifier is a mixture of salicylic acid, tartaric acid and malic acid; preferably, the acidic molecular modifier is a mixture of salicylic acid, tartaric acid and malic acid in a weight ratio of (30-60): (15-25): (5-55).

3. The acid-base modified corrosion-resistant coal gasification slag filling material according to claim 1, characterized in that: The nanocomposite emulsion is a mixture of styrene acrylic emulsion, alcohol ester dodecahydrate and polyurethane; preferably, the nanocomposite emulsion comprises, by weight: 30-70 parts of styrene acrylic emulsion, 20-50 parts of alcohol ester dodecahydrate and 5-20 parts of polyurethane, and / or The particle size of the styrene acrylic emulsion or alcohol ester or polyurethane is less than 200nm.

4. The acid-base modified corrosion-resistant coal gasification slag filling material according to claim 1, characterized in that: The alkaline activator includes at least one of sodium hydroxide, potassium hydroxide and sodium silicate; preferably, the alkaline activator is a mixture of sodium hydroxide, potassium hydroxide and sodium silicate; preferably, the alkaline activator includes, by weight: 20-60 parts of sodium hydroxide, 5-20 parts of potassium hydroxide and 20-85 parts of sodium silicate; preferably, the sodium silicate is sodium silicate with a water glass modulus of 2.5-3.

5.

5. The acid-base modified corrosion-resistant coal gasification slag filling material according to claim 1, characterized in that: The particle size of the coal gasification slag powder is not greater than 200 μm, and / or The particle size of the coal gasification slag coarse aggregate is not higher than 30 mm; preferably, the particle size of the coal gasification slag coarse aggregate is 15-30 mm.

6. The method for preparing the acid-base modified corrosion-resistant coal gasification slag filling material according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, mixing the coal gasification slag powder and the acidic molecular modifier evenly, and putting them into a ball mill for ball milling to obtain a first mixed powder; S2, mixing the first mixed powder with slag, adding nanocomposite emulsion, and grinding in a ball mill to obtain a second mixed material; S3. Add alkali activator, water and coal gasification slag coarse aggregate into the second mixture, mix and stir to obtain filling material.

7. The method according to claim 6, characterized in that In step S1, the ball milling time is 15-45 minutes, and / or The rotation speed of the ball mill is 520 r / min.

8. The method according to claim 6, characterized in that In step S2, the first mixed powder is mixed with slag for 3-5 minutes, and / or Add the nanocomposite emulsion and mill in a ball mill for 15-40 minutes, and / or The rotation speed of the ball mill is 400 r / min.

9. The method according to claim 6, characterized in that In step S3, the order of adding alkali activator, water, and coal gasification slag coarse aggregate is to add alkali activator, water, and coal gasification slag coarse aggregate in sequence, and / or The alkali activator, water and coal gasification slag coarse aggregate are added and stirred for 5-10 minutes.

10. Use of the acid-base modified corrosion-resistant coal gasification slag filling material according to any one of claims 1 to 5 in the field of coal-based solid waste filling.

Citation Information

Patent Citations

  • Super-hydrophobic / super-oleophylic adsorbent prepared by taking coal gasification slag as raw material as well as preparation method and application of super-hydrophobic / super-oleophylic adsorbent

    CN115090264A

  • Polymer functional filler prepared from fine coal gasification slag as well as preparation method and application of polymer functional filler

    CN116063740A

  • Mine filling material based on coal gasification slag as well as preparation method and application thereof

    CN116143484A

  • Method for preparing cemented filling material by using desulfurized gypsum to excite coal gasification slag

    CN117229002A

  • Coal gasification slag-based alkali-activated self-cementing underground filling material and preparation method thereof

    CN117328935A

Cited By

  • Method for utilizing multiple components of coal gasification fine slag and constructing nano functional material

    CN121134787A