Composite cementing material, preparation method and application thereof, ultra-high performance concrete and preparation method thereof

By pretreating the incineration fly ash and incineration bottom slag, composite cementitious materials and ultra-high performance concrete are prepared, which solves the problem of incineration solid waste disposal, realizes resource utilization and improves mechanical properties, and solves the solids generated by incineration of urban domestic waste Problem of increasing waste.

CN118930179APending Publication Date: 2024-11-12SHANGHAI FUPEI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110030.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Proper disposal and resource utilization of incineration bottom slag and incineration fly ash have become urgent problems to be solved. With the increase in solid waste generated by incineration of urban domestic waste, it is difficult for the existing technology to effectively utilize these resources.

Method used

By pretreating the incineration fly ash and incineration bottom slag, composite cementitious materials and ultra-high performance concrete are prepared, and solid waste such as incineration fly ash, fly ash, incineration bottom slag is used as raw materials, combining cement, silicon powder, slag powder, etc. Components, high-performance concrete is prepared, cement consumption is reduced, production costs are saved, and resource utilization is realized.

Benefits of technology

The resource utilization of solid waste such as incineration fly ash and incinerator slag has been realized, which reduces the hydration heat and reduces production costs. The ultra-high performance concrete prepared has good mechanical properties and is suitable for large-scale production and transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993110660000011
    Figure BDA0004993110660000011
  • Figure BDA0004993110660000031
    Figure BDA0004993110660000031
  • Figure BDA0004993110660000041
    Figure BDA0004993110660000041
Patent Text Reader

Abstract

The invention belongs to the technical field of concrete, and particularly relates to a composite cementing material, a preparation method and application thereof, ultra-high performance concrete and a preparation method thereof. The solid wastes such as the incineration fly ash, the fly ash and the incineration bottom slag are used as raw materials of the ultra-high performance concrete, so that the consumption of cement is reduced, the hydration heat is reduced, the production cost of the ultra-high performance concrete is saved, and meanwhile, the resource utilization of the solid wastes such as the incineration fly ash and the incineration slag is realized. The composite cementing material and the ultra-high performance concrete mixed powder provided by the invention can be produced on a large scale in a factory, and the composite cementing material and the ultra-high performance concrete mixed powder are dry powder materials and are long in storage period and convenient to transport.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of concrete, and specifically relates to a composite cementitious material and a preparation method and application thereof, and ultra-high performance concrete and a preparation method thereof. Background Art

[0002] With the continuous advancement of urbanization, garbage disposal has become a serious environmental problem. Waste incineration is a common way of garbage disposal. The incineration method of urban domestic waste has the advantages of maximum reduction, harmlessness, and resource utilization. After incineration, urban domestic waste is divided into incineration bottom ash and incineration fly ash according to the different collection locations in the waste incineration system. Incineration bottom ash is mainly the residue collected on the furnace bed after the incineration of garbage, and incineration fly ash is mainly fine-grained powder collected in the flue gas purification system of the waste incinerator. Due to the increasing amount of urban domestic waste, the incineration bottom ash and fly ash generated by incineration are also gradually increasing. The proper disposal and resource utilization of incineration bottom ash and incineration fly ash have become urgent problems and important research directions. Summary of the invention

[0003] In view of this, the present invention provides a composite cementitious material and a preparation method and application thereof, an ultra-high performance concrete and a preparation method thereof. The present invention uses the incineration bottom ash and incineration fly ash produced by garbage incineration to prepare ultra-high performance concrete, thereby realizing the resource utilization of solid waste.

[0004] In order to solve the above technical problems, the present invention provides a composite cementitious material, comprising the following components in percentage by mass:

[0005]

[0006] The pretreatment method for pre-treating incineration fly ash comprises the following steps: washing, drying and grinding the incineration fly ash in sequence to obtain the pre-treated incineration fly ash.

[0007] Preferably, the average particle size of the cement is 35-45 μm, the average particle size of the pretreated incineration fly ash is 1-5 μm, the average particle size of the silica powder is 0.05-1 μm, the average particle size of the fly ash is 5-15 μm, and the D90 of the slag powder is less than or equal to 30 μm.

[0008] Preferably, the water reducer is a polycarboxylic acid high-efficiency water reducer;

[0009] The defoaming agent includes one or more of an organosilicon defoaming agent, a polyurethane defoaming agent and a silicate defoaming agent.

[0010] The present invention also provides a method for preparing the composite gelling material described in the above technical solution, comprising the following steps:

[0011] The composite cementitious material is obtained by mixing the cement, pre-treated incineration fly ash, silica powder, fly ash, slag powder, water reducing agent and defoaming agent.

[0012] Preferably, the mixing is performed under stirring conditions, the stirring speed is 60 to 75 rpm, and the stirring time is 8 to 12 min.

[0013] The present invention also provides the use of the composite cementitious material described in the above technical solution or the composite cementitious material prepared by the preparation method described in the above technical solution in the preparation of ultra-high performance concrete.

[0014] The present invention also provides an ultra-high performance concrete, comprising an ultra-high performance concrete mixed powder and water; the ultra-high performance concrete mixed powder comprises the following components in percentage by mass:

[0015] Composite cementitious materials 40-55%;

[0016] Aggregate 40-55%;

[0017] Steel fiber 2-5%;

[0018] The composite gelling material is the composite gelling material described in the above technical solution or the composite gelling material prepared by the preparation method described in the above technical solution;

[0019] The aggregates include quartz sand and pre-treated incineration ash;

[0020] The pretreatment method of the pretreated incineration bottom ash comprises the following steps: sequentially crushing, demetallizing, washing, drying and screening the incineration bottom ash to obtain the pretreated incineration bottom ash.

[0021] Preferably, the mass percentage of silicon dioxide in the quartz sand is more than 95%; the mass percentage of incineration bottom ash in the aggregate is 25-35%;

[0022] The aggregate includes first particle size aggregate, second particle size aggregate, third particle size aggregate and fourth particle size aggregate; the particle size of the first particle size aggregate is greater than or equal to 10 mesh and less than 30 mesh, the particle size of the second particle size aggregate is greater than or equal to 30 mesh and less than 60 mesh, the particle size of the third particle size aggregate is greater than or equal to 60 mesh and less than 90 mesh, and the particle size of the fourth particle size aggregate is greater than or equal to 90 mesh and less than 120 mesh.

[0023] Preferably, the steel fiber has a diameter of 0.12 to 0.25 mm and a length of 10 to 19 mm;

[0024] The water-cement ratio of the ultra-high performance concrete is 0.15-0.20.

[0025] The present invention also provides a method for preparing the ultra-high performance concrete described in the above technical solution, comprising the following steps:

[0026] The composite cementitious material, aggregate and steel fiber are first mixed to obtain ultra-high performance concrete mixed powder;

[0027] The mixed powder and water are mixed for a second time to obtain the ultra-high performance concrete.

[0028] The invention provides a composite cementitious material, comprising the following components in percentage by mass: 50-60% cement, 5-15% pre-treated incineration fly ash, 3-10% silica powder, 10-20% fly ash, 10-20% slag powder, 0.5-1.5% water reducing agent and 0.01-0.15% defoaming agent; the pre-treatment method of the pre-treated incineration fly ash comprises the following steps: washing, drying and grinding the incineration fly ash in sequence to obtain the pre-treated incineration fly ash. The present invention also provides an ultra-high performance concrete comprising an ultra-high performance concrete mixed powder and water; the ultra-high performance concrete mixed powder comprises the following components in percentage by mass: 40-55% composite cementitious material, 40-55% aggregate, and 2-5% steel fiber; the composite cementitious material is the composite cementitious material described in the above technical solution or the composite cementitious material prepared by the preparation method described in the above technical solution; the aggregate comprises quartz sand and pre-treated incineration bottom ash; the pretreatment method of the pre-treated incineration bottom ash comprises the following steps: the incineration bottom ash is sequentially crushed, demetallized, washed, dried and screened to obtain the pre-treated incineration bottom ash. The present invention utilizes solid wastes such as incineration fly ash, fly ash, and incineration bottom ash as raw materials for ultra-high performance concrete, saves the amount of cement, reduces the hydration heat, and realizes the resource utilization of solid wastes such as incineration fly ash and incineration slag while saving the production cost of ultra-high performance concrete. The composite cementitious material and ultra-high performance concrete mixed powder provided by the present invention can be mass-produced in a factory, and the composite cementitious material and ultra-high performance concrete mixed powder are dry powders with a long storage period and are easy to transport. DETAILED DESCRIPTION

[0029] The present invention provides a composite cementitious material, comprising the following components in percentage by weight:

[0030]

[0031]

[0032] The pretreatment method for pre-treating incineration fly ash comprises the following steps: washing, drying and grinding the incineration fly ash in sequence to obtain the pre-treated incineration fly ash.

[0033] In terms of mass percentage, the composite cementitious material provided by the present invention comprises 50-60% cement, preferably 52-58%, and more preferably 55-56%. In the present invention, the average particle size of the cement is preferably 35-45 μm, and more preferably 40 μm. In the present invention, the cement is preferably ordinary Portland cement, and more preferably 52.5 grade ordinary Portland cement.

[0034] In terms of mass percentage, the composite cementitious material provided by the present invention comprises 5-15% pre-treated incineration fly ash, preferably 10-14%, and more preferably 12%. In the present invention, the average particle size of the pre-treated incineration fly ash is preferably 1-5 μm, and more preferably 2-4 μm. In the present invention, the pretreatment method of the pre-treated incineration fly ash comprises the following steps: washing, drying and grinding the incineration fly ash in sequence to obtain the pre-treated incineration fly ash. In the present invention, the incineration fly ash comprises soluble salt, SiO2, CaO, Al2O3, MgO and Fe2O3. In the present invention, the soluble salt is preferably one or more of sodium chloride, potassium chloride and calcium chloride; the mass percentage of the soluble salt in the incineration fly ash is preferably 10-20%, and more preferably 11.89-15%. In the present invention, the high content of chloride ions in the soluble salt is not conducive to the comprehensive utilization of the incineration fly ash. The present invention can remove soluble salts in the incineration fly ash through water washing, so that the content of chloride ions in the pre-treated incineration fly ash is reduced to 0.59-0.8%. In the present invention, the incineration fly ash after water washing preferably includes SiO225.6%, CaO 24.3%, Al2O34.7%, MgO 1.8%, and Fe2O35.9% in terms of mass percentage. In the present invention, the drying is preferably drying. The present invention has no special restrictions on the drying, as long as the surface moisture can be removed. In the present invention, the rotation speed of the grinding is preferably 45-50r / min, more preferably 48r / min; the grinding time is preferably 18-22min, more preferably 20min. In the present invention, the grinding is preferably carried out in a QM-480-600 horizontal high-fine grinding test machine. In the present invention, after the grinding, it is preferred to further include: air separation and classification of the ground product to obtain pre-treated incineration fly ash with an average particle size of 1-5μm. In the present invention, the air selection and classification are preferably carried out in an OS-Ⅰ type superfine classifier, and the rotor linear speed of the OS-Ⅰ type superfine classifier is preferably 90-110 m / s, more preferably 100 m / s; the time for the air selection and classification is preferably 0.8-1.2 h, more preferably 1 h.

[0035] The composite cementitious material provided by the present invention comprises 3-10% silicon micropowder, preferably 5-8%, more preferably 6%, by mass percentage. In the present invention, the average particle size of the silicon micropowder is preferably 0.05-1 μm, more preferably 0.1-0.8 μm.

[0036] In the present invention, the silicon micropowder as an ultrafine active mineral admixture can reduce the porosity, optimize the pore structure, and improve the density between cementitious materials. The prepared composite cementitious material is suitable for ultra-high performance concrete.

[0037] In terms of mass percentage, the composite cementitious material provided by the present invention includes 10-20% fly ash, preferably 13-15%. In the present invention, the average particle size of the fly ash is preferably 5-15 μm, more preferably 8-12 μm. In the present invention, the commercially available secondary fly ash is preferably ground, air-selected and classified to obtain fly ash with an average particle size of 5-15 μm. In the present invention, the rotation speed of the grinding is preferably 45-50 r / min, more preferably 48 r / min; the grinding time is preferably 8-12 min, more preferably 10 min. In the present invention, the grinding is preferably carried out in a QM-480-600 horizontal high-fine grinding test machine. In the present invention, the air selection and classification are preferably carried out in an OS-Ⅰ type superfine classifier, and the rotor linear speed of the OS-Ⅰ type superfine classifier is preferably 90-110 m / s, more preferably 100 m / s; the air selection and classification time is preferably 0.8-1.2 h, more preferably 1 h.

[0038] In the present invention, the fly ash as an ultrafine active mineral admixture can reduce porosity, optimize pore structure, and improve the density between cementitious materials. The prepared composite cementitious material is suitable for ultra-high performance concrete.

[0039] In terms of mass percentage, the composite cementitious material provided by the present invention includes 10-20% slag powder, preferably 13-16%. In the present invention, the average particle size of the slag powder is preferably less than or equal to 30 μm, more preferably 20-26 μm. In the present invention, S95 grade slag powder, grinding aid and activator are preferably mixed and ground to obtain slag powder with an average particle size of less than or equal to 30 μm. In the present invention, the grinding aid is preferably a mixture of triethanolamine, isopropanol and wood calcium. Based on the total amount of slag powder, the addition amount of triethanolamine is preferably 0.1-0.5‰, the addition amount of isopropanol is preferably 0.1-0.3‰, and the addition amount of wood calcium is preferably 0.6-3‰. In the present invention, the addition amount of the grinding aid is preferably 1-3‰ of the weight of the slag powder. In the present invention, the activator is preferably a mixed powder of desulfurized gypsum, nano-silicon dioxide and sodium sulfate. Based on the total amount of slag powder, the addition amount of desulfurized gypsum (calcium sulfate) is preferably 10-15%, the addition amount of nano-silicon dioxide is preferably 0.1-0.3‰, and the addition amount of sodium sulfate is preferably 0.1-0.5‰. The present invention has no special requirements on the particle size of the nano-silicon dioxide, as long as it is nanometer; in the present invention, the average particle size of the desulfurized gypsum is preferably 40-50μm, and the average particle size of the sodium sulfate is preferably 40-50μm. In the present invention, the addition amount of the activator is 5-15% of the weight of the slag powder.

[0040] In the present invention, the grinding time is preferably 10 to 15 minutes. The present invention has no special requirements on the grinding speed, as long as the prism-like physical appearance of the slag powder can be changed to a spherical type. In the present invention, the specific surface area of ​​the slag powder is preferably 480 to 520 m 2 / kg, more preferably 500m 2 The present invention limits the particle size of the slag powder to the above range to have a larger specific surface area, thereby improving its activity.

[0041] The composite cementitious material provided by the present invention comprises 0.5-1.5% water reducer, preferably 0.9-1.1% by mass percentage. In the present invention, the water reducer is preferably a polycarboxylic acid high-efficiency water reducer, and the water reducer is preferably a powder. In the present invention, the water reduction rate of the water reducer is preferably greater than 35%.

[0042] In terms of mass percentage, the composite gelling material provided by the present invention comprises 0.01-0.15% defoamer, preferably 0.1-0.12%. In the present invention, the defoamer is preferably a powder. In the present invention, the defoamer preferably comprises one or more of an organosilicon defoamer, a polyurethane defoamer and a silicate defoamer, more preferably one of an organosilicon defoamer, a polyurethane defoamer and a silicate defoamer, and further preferably an organosilicon defoamer.

[0043] The present invention limits the particle size of silicon micropowder, pre-treated incineration fly ash, pulverized coal, slag powder and cement to the above range, so that the particle size composition of silicon micropowder, pre-treated incineration fly ash, pulverized coal, slag powder and cement has a reasonable particle gradation, thereby achieving mutual filling.

[0044] The present invention also provides a method for preparing the composite gelling material described in the above technical solution, comprising the following steps:

[0045] The composite cementitious material is obtained by mixing the cement, pre-treated incineration fly ash, silica powder, fly ash, slag powder, water reducing agent and defoaming agent.

[0046] In the present invention, cement, pre-treated incineration fly ash, silica powder, fly ash, slag powder, water reducing agent and defoaming agent are preferably added to a mixing device in sequence for mixing. In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring speed is preferably 60 to 75 rpm, more preferably 65 to 70 rpm; the stirring time is preferably 8 to 12 minutes, more preferably 10 minutes.

[0047] The present invention also provides the use of the composite cementitious material described in the above technical solution or the composite cementitious material prepared by the preparation method described in the above technical solution in the preparation of ultra-high performance concrete.

[0048] The present invention also provides an ultra-high performance concrete, comprising an ultra-high performance concrete mixed powder and water; the ultra-high performance concrete mixed powder comprises the following components in percentage by mass:

[0049] Composite cementitious materials 40-55%;

[0050] Aggregate 40-55%;

[0051] Steel fiber 2-5%;

[0052] The composite gelling material is the composite gelling material described in the above technical solution or the composite gelling material prepared by the preparation method described in the above technical solution.

[0053] Calculated by mass percentage, the ultra-high performance concrete mixed powder provided by the present invention includes 40-55% of composite cementitious materials, preferably 45-50%.

[0054] In terms of mass percentage, the ultra-high performance concrete mixed powder provided by the present invention comprises 40-55% aggregate, preferably 42-52%, and more preferably 47-50%. In the present invention, the aggregate preferably comprises quartz sand and pre-treated incineration bottom ash. In the present invention, the mass percentage of silicon dioxide in the quartz sand is preferably above 95%, and more preferably 96-98%.

[0055] In the present invention, the pretreatment method of the pretreated incineration bottom ash comprises the following steps: the incineration bottom ash is sequentially crushed, demetallized, washed, dried and screened to obtain the pretreated incineration bottom ash. In the present invention, after the classified recycling of domestic waste, there is very little glass, iron and other metals before the waste incineration. Incineration bottom ash is the solid residue of the molten material produced in the process of waste incineration, and its composition is mainly SiO2, Al2O3, CaO, MgO, etc., and it also contains other metals such as iron, aluminum, and copper. Since the main physical components of the slag are hard in texture, it can be guaranteed to have a certain strength when used as aggregate. In the present invention, the demetallization treatment preferably comprises the following steps:

[0056] The incineration bottom ash is subjected to a first crushing and then a first magnetic separation to obtain the iron-removed bottom ash;

[0057] The de-ironized bottom ash is subjected to a first eddy current sorting to separate non-iron metals to obtain primary pre-treated incineration bottom ash;

[0058] The primary pretreated incineration bottom ash is subjected to a second crushing and then sequentially subjected to a second magnetic separation and a second eddy current separation to obtain the pretreated incineration bottom ash.

[0059] In the present invention, the average particle size of the first crushed product is preferably 8 to 12 mm, more preferably 10 mm. The present invention has no special requirements for the first magnetic separation, and a conventional method in the art can be used. The present invention has no special requirements for the first eddy current separation, and a conventional method in the art can be used.

[0060] In the present invention, the average particle size of the second crushed product is preferably 4 to 6 mm, more preferably 5 mm. The present invention has no special requirements for the second magnetic separation, and a conventional method in the art can be used. The present invention has no special requirements for the second eddy current separation, and a conventional method in the art can be used.

[0061] The present invention has no special requirements for the crushing, washing, drying and screening, as long as the incineration bottom ash with particle sizes greater than or equal to 10 mesh and less than 30 mesh, greater than or equal to 30 mesh and less than 60 mesh, greater than or equal to 60 mesh and less than 90 mesh, and greater than or equal to 90 mesh and less than 120 mesh can be obtained.

[0062] In the present invention, the mass percentage of the incineration bottom ash in the aggregate is preferably 25-35%, more preferably 27-30%.

[0063] In the present invention, the aggregate preferably includes first particle size aggregate, second particle size aggregate, third particle size aggregate and fourth particle size aggregate; the particle size of the first particle size aggregate is preferably greater than or equal to 10 mesh and less than 30 mesh, the particle size of the second particle size aggregate is preferably greater than or equal to 30 mesh and less than 60 mesh, the particle size of the third particle size aggregate is preferably greater than or equal to 60 mesh and less than 90 mesh, and the particle size of the fourth particle size aggregate is preferably greater than or equal to 90 mesh and less than 120 mesh. In the present invention, the mass ratio of the first particle size aggregate, the second particle size aggregate, the third particle size aggregate and the fourth particle size aggregate is preferably 1:1:1:1.

[0064] The present invention limits the particle size of aggregates within the above range to form a reasonable particle gradation and fill each other; the composite cementitious material and aggregate, the particles of different particle sizes of the constituent materials form the most dense stacking in the best ratio, that is, the gaps between the stacking of millimeter-level particles (aggregates) are filled with micron-level particles (cement, incineration fly ash, pulverized coal powder, slag powder), and the gaps between the stacking of micron-level particles are filled with submicron-level particles (silicon powder), forming the most dense stacking, so that the ultra-high performance concrete material has the best particle grading, better micro-powder filling effect, can further reduce the porosity, and optimize the internal pore structure, so as to achieve dense stacking of the matrix.

[0065] In the present invention, the aggregate complies with the standard of GB / T25032-2010 "Aggregate of slag from the incineration of domestic waste", has the characteristics of good firmness, relatively stable chemical properties, good durability, and certain strength, and can meet the requirements of aggregate utilization.

[0066] The ultra-high performance concrete mixed powder provided by the present invention comprises 2-5% steel fiber, preferably 3-4%, by mass percentage. In the present invention, the diameter of the steel fiber is preferably 0.12-0.25 mm, more preferably 0.15-0.2 mm; the length of the steel fiber is preferably 10-19 mm, more preferably 13-17 mm. In the present invention, the steel fiber can improve the ductility of ultra-high performance concrete.

[0067] In the present invention, the water-cement ratio of the ultra-high performance concrete is preferably 0.15 to 0.20, and more preferably 0.17 to 0.19.

[0068] The present invention also provides a method for preparing the ultra-high performance concrete described in the above technical solution, comprising the following steps:

[0069] The composite cementitious material, aggregate and steel fiber are first mixed to obtain ultra-high performance concrete mixed powder;

[0070] The mixed powder and water are mixed for a second time to obtain the ultra-high performance concrete.

[0071] The present invention performs a first mixing of the composite cementitious material, aggregate and steel fiber to obtain the ultra-high performance concrete mixed powder. In the present invention, the first mixing is preferably performed under stirring conditions, and the stirring speed is preferably 50 to 60 r / min, more preferably 55 to 60 r / min; the stirring time is preferably 4 to 6 min, more preferably 5 min. In the present invention, the stirring is preferably performed in a mixer.

[0072] After obtaining the ultra-high performance concrete mixed powder, the present invention performs a second mixing of the mixed powder and water to obtain the ultra-high performance concrete. In the present invention, the second mixing is preferably performed under stirring conditions, and the stirring speed is preferably 45 to 55 r / min, more preferably 50 r / min; the stirring time is preferably 8 to 10 min, more preferably 9 min. In the present invention, the stirring is preferably performed in a vertical axis planetary mixer.

[0073] The present invention performs a second mixing of the ultra-high performance concrete mixed powder and water before use to obtain ultra-high performance concrete. In the present invention, the ultra-high performance concrete is preferably cured at room temperature. In the present invention, the room temperature is preferably 5 to 40°C, more preferably 20 to 35°C, and further preferably 25 to 30°C. In the present invention, the initial expansion of the ultra-high performance concrete is preferably 700 to 730 mm, the 3d compressive strength is preferably 70 to 100 MPa, the 28d compressive strength is preferably 120 to 150 MPa, the ultimate tensile strength is preferably 8 to 10 MPa, and the ultimate tensile strain is preferably 0.2 to 0.3%.

[0074] In the present invention, particles of different particle sizes of composite cementitious materials and aggregates in the ultra-high performance concrete form the most compact stacking in an optimal ratio, that is, the gaps between the stacking of millimeter-level particles (aggregates) are filled with micron-level particles (cement, incineration fly ash, pulverized coal powder, slag powder), and the gaps between the stacking of micron-level particles are filled with submicron-level particles (silicon powder), forming the most compact stacking, so that the ultra-high performance concrete material of the invention has a more reasonable particle grading, better powder filling effect, can further reduce porosity, and has a more optimized internal pore structure, so that these particles and admixtures can achieve a close stacking of the matrix and a strong molecular binding force through proper mixing, pouring and room temperature curing.

[0075] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0076] Example 1

[0077] The ingredients are weighed according to the ratio, and the amount of each raw material is: 52kg of 52.5 grade ordinary Portland cement with an average particle size of 40μm, 14kg of pretreated incineration fly ash with an average particle size of 3μm, 8kg of silica powder with an average particle size of 0.5μm, 15kg of fly ash with an average particle size of 10μm, 10kg of slag powder with an average particle size of 25μm, 0.9kg of polycarboxylic acid water reducer (water reduction rate greater than 35%), and 0.1kg of silicone defoaming agent.

[0078] The incineration fly ash with a chloride ion content of 11.89% is subjected to water washing and desalination treatment to obtain a water-washed incineration fly ash with a chloride ion content of 0.59%, SiO2 25.6wt%, CaO 24.3wt%, Al2O3 4.7wt%, MgO 1.8wt%, and Fe2O3 5.9wt%; the water-washed incineration fly ash is dried and then put into a QM-480-600 horizontal high-fine grinding test machine for grinding at a speed of 48r / min for 20min; the ground incineration fly ash is then put into an OS-Ⅰ type superfine classifier, the rotor linear speed is adjusted to 100m / s, the automatic feeding button is started, and air selection and classification are carried out for 1h to obtain pre-treated incineration fly ash with a particle size of 3μm;

[0079] Pretreatment of fly ash: put the commercially available secondary fly ash into the QM-480-600 horizontal high-fine grinding test machine and grind it at a speed of 48r / min for 10min; then put the ground fly ash into the OS-Ⅰ type superfine classifier, adjust the rotor linear speed to 100m / s, start the automatic feeding button, and carry out air separation and classification. After 1h, fly ash with a particle size of 10μm is obtained;

[0080] Pretreatment of slag powder: grind the commercially available slag powder to a specific surface area of ​​400m 2 / kg of S95 grade slag powder was introduced into the horizontal ball mill. Grinding aids and activators were sprayed into the ball mill during grinding. After grinding for 13 minutes, a specific surface area of ​​500m 2 / kg of slag powder; wherein the grinding aid is a mixture of triethanolamine, isopropanol and wood calcium, the grinding aid is added in an amount of 1.5‰ of the weight of the slag powder, wherein the triethanolamine is added in an amount of 0.3‰ of the weight of the slag powder, the isopropanol is added in an amount of 0.2‰ of the weight of the slag powder, and the wood calcium is added in an amount of 1‰ of the weight of the slag powder; the activator is a mixed powder of desulfurized gypsum (with an average particle size of 45μm), nano-silicon dioxide and sodium sulfate (with an average particle size of 45μm), the activator is added in an amount of 15% of the weight of the slag powder, wherein the desulfurized gypsum is added in an amount of 14.95% of the weight of the slag powder, the nano-silicon dioxide is added in an amount of 0.2‰ of the weight of the slag powder, and the sodium sulfate is added in an amount of 0.3‰ of the weight of the slag powder;

[0081] Put 52.5 grade ordinary Portland cement, pre-treated incineration fly ash, silica powder, fly ash, slag powder, water reducing agent and defoaming agent into a mixer in sequence and stir at a speed of 70r / min for 10min to obtain a composite cementitious material;

[0082] Weigh the ingredients according to the ratio, the amount of each raw material is:

[0083] 45kg of composite cementitious material, 52kg of aggregate (including 37.44kg of quartz sand and 14.56kg of pre-treated incineration ash), and 3kg of steel fiber with a diameter of 0.2mm and a length of 15mm.

[0084] The content of silicon dioxide in the quartz sand is greater than 95%, and the particle sizes are greater than or equal to 10 mesh and less than 30 mesh, greater than or equal to 30 mesh and less than 60 mesh, greater than or equal to 60 mesh and less than 90 mesh, and greater than or equal to 90 mesh and less than 120 mesh. The dosage of quartz sand with different particle sizes is 9.36 kg;

[0085] Incineration bottom ash pretreatment method: the incineration bottom ash is crushed by a crusher to obtain incineration bottom ash with a particle size of 10mm, and then magnetic separation is performed to obtain iron-free bottom ash; the iron-free bottom ash is placed in a crusher for eddy current separation and then crushed to obtain bottom ash with a particle size of 5mm; the crushed bottom ash is subjected to mechanical magnetic separation and eddy current separation again, and then washed, dried and vibrated screened in turn to obtain pretreated incineration bottom ash with particle sizes greater than or equal to 10 mesh and less than 30 mesh, greater than or equal to 30 mesh and less than 60 mesh, greater than or equal to 60 mesh and less than 90 mesh, and greater than or equal to 90 mesh and less than 120 mesh, and the dosage of pretreated incineration bottom ash with different particle sizes is 3.64kg;

[0086] The composite cementitious material powder, aggregate and steel fiber are sequentially placed into a mixer and stirred at a speed of 60 r / min for 5 minutes to obtain an ultra-high performance concrete mixed powder.

[0087] The ultra-high performance concrete mixed powder was put into a vertical axis planetary mixer, 8.55 kg of water was added, and the mixture was stirred at a speed of 50 r / min for 10 min to obtain an ultra-high performance concrete with a water-cement ratio of 0.19.

[0088] Example 2

[0089] The composite cementitious material was prepared according to the method of Example 1, except that the types and amounts of raw materials used in preparing the composite cementitious material were: 55 kg of 52.5 grade ordinary cement, 12 kg of pre-treated incineration fly ash, 6 kg of silica powder, 13 kg of fly ash, 13 kg of slag powder, 0.9 kg of polycarboxylic acid water reducer, and 0.1 kg of polyurethane defoamer;

[0090] 52.5 grade ordinary cement, pre-treated incineration fly ash, silica powder, fly ash, slag powder, water reducing agent and defoaming agent are sequentially placed in a mixer and stirred at a speed of 68 r / min for 10 min to obtain a composite cementitious material;

[0091] Ultra-high performance concrete was prepared according to the method of Example 1, except that the amount of mixed powder used to prepare the ultra-high performance concrete was: 50 kg of composite cementitious material, 47 kg of aggregate (including 32.9 g of quartz sand and 14.1 kg of pretreated incineration bottom ash), and 3 kg of steel fiber; the amount of quartz sand of different particle sizes was 8.225 kg, and the amount of incineration bottom ash of different particle sizes was 3.525 kg; the amount of water added was 9 kg to obtain an ultra-high performance concrete with a water-cement ratio of 0.18.

[0092] Example 3

[0093] The composite cementitious material was prepared according to the method of Example 1, except that the types and amounts of raw materials used in preparing the composite cementitious material were: 58 kg of 52.5 grade ordinary cement, 10 kg of pre-treated incineration fly ash, 5 kg of silica powder, 10 kg of fly ash, 16 kg of slag powder, 0.9 kg of polycarboxylate water reducer, and 0.1 kg of silicate defoamer;

[0094] 52.5 grade ordinary cement, pre-treated incineration fly ash, silica powder, fly ash, slag powder, water reducing agent and defoaming agent are sequentially placed in a mixer and stirred at a speed of 68 r / min for 10 min to obtain a composite cementitious material;

[0095] Ultra-high performance concrete was prepared according to the method of Example 1, except that the amount of mixed powder used to prepare the ultra-high performance concrete was: 55 kg of composite cementitious material, 42 kg of aggregate (including 27.3 kg of quartz sand and 14.7 kg of pre-treated incineration bottom ash), and 3 kg of steel fiber; the amount of quartz sand of different particle sizes was 6.825 kg, and the amount of incineration bottom ash of different particle sizes was 3.675 kg; the amount of water added was 9.35 kg to obtain an ultra-high performance concrete with a water-cement ratio of 0.17.

[0096] The ultra-high performance concrete prepared in Examples 1 to 3 was subjected to performance tests after curing at room temperature, and the results are listed in Table 1.

[0097] Table 1 Performance of ultra-high performance concrete prepared in Examples 1 to 3

[0098]

[0099] It can be seen from the test results in Table 1 that the ultra-high performance concrete provided by the present invention has good mechanical properties. The present invention prepares ultra-high performance concrete using solid wastes such as incineration fly ash and incineration bottom slag as raw materials, thereby realizing the resource utilization of solid waste.

[0100] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A composite gelling material, characterized in that: Includes the following components in percentage by mass: The pretreatment method for pre-treating incineration fly ash comprises the following steps: washing, drying and grinding the incineration fly ash in sequence to obtain the pre-treated incineration fly ash.

2. The composite gelling material according to claim 1, characterized in that: The average particle size of the cement is 35-45 μm, the average particle size of the pretreated incineration fly ash is 1-5 μm, the average particle size of the silicon micropowder is 0.05-1 μm, the average particle size of the fly ash is 5-15 μm, and the D90 of the slag powder is less than or equal to 30 μm.

3. The composite cementitious material according to claim 1, characterized in that: The water reducer is a polycarboxylic acid high-efficiency water reducer; The defoaming agent includes one or more of an organosilicon defoaming agent, a polyurethane defoaming agent and a silicate defoaming agent.

4. The method for preparing the composite gelling material according to any one of claims 1 to 3, comprising the following steps: The composite cementitious material is obtained by mixing the cement, pre-treated incineration fly ash, silica powder, fly ash, slag powder, water reducing agent and defoaming agent.

5. The preparation method according to claim 4, characterized in that: The mixing is carried out under stirring conditions, the stirring speed is 60 to 75 rpm, and the stirring time is 8 to 12 minutes.

6. Use of the composite cementitious material according to any one of claims 1 to 3 or the composite cementitious material prepared by the preparation method according to claim 4 or 5 in the preparation of ultra-high performance concrete.

7. An ultra-high performance concrete, characterized in that: The ultra-high performance concrete mixed powder and water are included; the ultra-high performance concrete mixed powder includes the following components in percentage by mass: Composite cementitious materials 40-55%; Aggregate 40-55%; Steel fiber 2-5%; The composite gelling material is the composite gelling material according to any one of claims 1 to 3 or the composite gelling material prepared by the preparation method according to claim 4 or 5; The aggregate includes quartz sand and pre-treated incineration bottom ash; The pretreatment method of the pretreated incineration bottom ash comprises the following steps: sequentially crushing, demetallizing, washing, drying and screening the incineration bottom ash to obtain the pretreated incineration bottom ash.

8. The ultra-high performance concrete according to claim 7, characterized in that: The mass percentage of silicon dioxide in the quartz sand is more than 95%; the mass percentage of incineration bottom ash in the aggregate is 25-35%; The aggregate includes first particle size aggregate, second particle size aggregate, third particle size aggregate and fourth particle size aggregate; the particle size of the first particle size aggregate is greater than or equal to 10 mesh and less than 30 mesh, the particle size of the second particle size aggregate is greater than or equal to 30 mesh and less than 60 mesh, the particle size of the third particle size aggregate is greater than or equal to 60 mesh and less than 90 mesh, and the particle size of the fourth particle size aggregate is greater than or equal to 90 mesh and less than 120 mesh.

9. The ultra-high performance concrete according to claim 7, characterized in that: The steel fiber has a diameter of 0.12 to 0.25 mm and a length of 10 to 19 mm; The water-cement ratio of the ultra-high performance concrete is 0.15-0.

20.

10. The method for preparing the ultra-high performance concrete according to any one of claims 7 to 9, comprising the following steps: The composite cementitious material, aggregate and steel fiber are first mixed to obtain ultra-high performance concrete mixed powder; The mixed powder and water are mixed for a second time to obtain the ultra-high performance concrete.