Strontium titanate-based giant dielectric ceramic material doped with simultaneous donors of Lu and Ta and preparation method of strontium titanate-based giant dielectric ceramic material
By using the simultaneous doping technology of Lu and Ta in SrTiO3-based materials, stable defect clusters and oxygen vacancies are formed, which solves the problem of limited improvement in dielectric performance of SrTiO3-based ceramics, and achieves significant improvement in dielectric constant and dielectric loss. The reduction meets the dielectric material needs of electronic components and energy storage devices, and reduces production costs.
Patent Information
- Application Number
- CN202411170468.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The dielectric performance improvement of existing SrTiO3-based giant dielectric ceramic materials is limited, making it difficult to meet the demand for dielectric materials by electronic components and energy storage devices, especially the problems of low dielectric constant and high dielectric loss.
Using the method of donor doping between Lu and Ta at the same time, doping at the A(Sr) and B(Ti) positions of SrTiO3 respectively. By forming stable defect clusters and oxygen vacancies, the dielectric constant of the material is increased and the dielectric loss is reduced. , a ceramic material with a huge dielectric effect was prepared by using a nitrogen sintering process.
It has achieved a significant increase in the dielectric constant and a reduction in dielectric loss, and has good frequency and temperature stability of dielectric performance, which meets the needs of electronic components and energy storage devices, and reduces production costs.
Smart Images

Figure CN118930252A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic functional materials, and in particular to a strontium titanate-based giant dielectric ceramic material doped with Lu and Ta as donors at the same time and a preparation method thereof. Background Art
[0002] Giant dielectric ceramics are widely used in the miniaturization of electronic devices. Common giant dielectric ceramics include TiO2-based, NiO-based, CaCu3Ti4O 12 Based on, BaTiO3 based and SrTiO3 based ceramics. Although these ceramic materials have been widely studied and reported, their applications are affected by the defects of the materials themselves. For example, the application of TiO2 based ceramics is limited by its low breakdown strength (5-10kV / mm); NiO based ceramics and CaCu3Ti4O 12 BaTiO3-based ceramics are limited by the difficulty in reducing dielectric loss (>0.1); BaTiO3-based ceramics will undergo a ferroelectric phase transition at the Curie temperature (~125℃), causing its dielectric constant to increase sharply to ~10000, which will affect its application under high temperature conditions. Compared with the above ceramics, SrTiO3-based ceramics have attracted attention due to their advantages such as high breakdown strength (~25kV / mm), low dielectric loss (~0.005) and low frequency and temperature dependence. However, pure SrTiO3 has the problem of low intrinsic dielectric constant (~300). Therefore, improving the dielectric properties of SrTiO3-based ceramics has extremely important application significance.
[0003] Doping modification and non-oxidizing atmosphere sintering can effectively improve the dielectric constant of SrTiO3-based giant dielectric ceramics. For example, Wang et al. (ZJWang, MHCao, ZHYao, Q.Zhang, Z.Song, W.Hu, Q.Xu, H.Hao, HXLiu, ZYYu, Giant permittivity and low dielectric loss of SrTiO3ceramics sinteredin nitrogen atmosphere, J.Eur.Ceram.Soc.34(2014)1755-1760.) reported that pure SrTiO3 ceramics sintered in nitrogen atmosphere have a giant dielectric constant (ε r ~47601) and low dielectric loss (tanδ~0.0058). And its dielectric constant shows a platform in the range of -100~200℃, which indicates that the temperature stability of the dielectric constant is good. Giant dielectric effect and defect dipole clusters generated by complete ionization of oxygen vacancies Doping modification also helps to improve the dielectric properties of SrTiO3. Especially for SrTiO3 with ABO3 cubic perovskite structure, ion doping modification at different sites will affect the type of defects, thereby affecting its dielectric properties. Qiao et al. (Qiao Y, Li W, Zhang Y, et al. Hole-pinned defect-dipoles induced colossal permittivity in Bi doped SrTiO3 ceramics with Sr deficiency [J]. Journal of Materials Science & Technology, 2020, 44: 54-61.) prepared Sr by A-site doping. 1-1.5x Bi x TiO3 (x = 0, 0.01, 0.05 and 0.1) ceramics can obtain giant dielectric effect when sintered in air atmosphere. When x = 0.05, the ceramic obtains ε r ~10 4 The giant dielectric constant and low dielectric loss of tanδ<0.05. Phase structure analysis and density functional theory calculations show that the pinning effect on free electrons Defect clusters are the main reason for the giant dielectric effect. Guo et al. (Guo X, Pu Y, Wang W, et al. Colossal permittivity and low dielectric loss in Ta dopedstrontium titanate ceramics by designing defect chemistry [J]. Journal of Alloys and Compounds, 2020, 818: 152866.) prepared SrTi by using Ta element donor doping at the B site. 1- x Ta x O3 ceramics (0.000≤x≤0.014) ceramics. The results show that in the ceramic sample with x=0.010, the giant dielectric constant (ε r The improvement in dielectric properties is related to the electron pinning defect dipole (EPDD) effect, which increases the dielectric constant by enhancing local polarization and suppresses the long-range displacement of electrons, thereby reducing dielectric loss over a wide frequency range.
[0004] However, the above studies are all single-element doping modifications, which have limited improvement on the dielectric properties of ceramic materials and are difficult to meet the demand for dielectric materials for miniaturization of electronic components and energy storage devices. Summary of the invention
[0005] In view of this, the present invention provides a method for preparing a Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material. The present invention uses Lu and Ta to simultaneously donor-dope the A (Sr) position and the B (Ti) position of SrTiO3, respectively. The obtained SrTiO3-based giant dielectric ceramic material has a giant dielectric effect, small dielectric loss, and good frequency and temperature stability of the dielectric constant, which meets the needs of miniaturization of electronic components and energy storage devices for dielectric materials.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A method for preparing a Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material comprises the following steps:
[0008] (1) SrCO3, TiO2, Lu2O3 and Ta2O5 are ball-milled once according to the stoichiometric ratio in formula I, and the ball-milled material obtained is dried and then synthesized to obtain a synthetic powder;
[0009] Sr 0.01 Lu 0.985 Ti 1-x Ta x O3 formula I;
[0010] In formula I: 0<x≤0.015;
[0011] (2) ball-milling the synthetic powder for a second time, followed by sieving and drying in sequence to obtain a second ball-milled material;
[0012] (3) mixing the secondary ball mill material, a binder and water, and then performing aging, granulation and dry pressing in sequence to obtain a ceramic body;
[0013] (4) Debinding and sintering the ceramic body in sequence to obtain the Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material; the sintering atmosphere is nitrogen.
[0014] Preferably, the conditions of the primary ball milling and the secondary ball milling independently include: the ball milling speed is 250-350 rpm, the ball milling time is 5-7 hours, and the ball milling medium is deionized water.
[0015] Preferably, the synthesis temperature is 1150-1250° C., the insulation time is 3-5 hours; the heating rate to the synthesis temperature is 4-6° C. / min; the synthesis atmosphere is air.
[0016] Preferably, the binder is a polyvinyl alcohol solution, and the concentration of the polyvinyl alcohol solution is 3-5wt.%; the amount of the binder is 1-2% of the mass of the synthetic powder; and the amount of water is 0.5-1% of the mass of the synthetic powder.
[0017] Preferably, the dry pressing pressure is 13-17 MPa; the diameter of the ceramic body is 8-12 mm, and the thickness is 1-2 mm.
[0018] Preferably, the debinding temperature is 550-650° C., and the holding time is 1.5-2.5 h.
[0019] Preferably, the sintering temperature is 1500-1550° C., the holding time is 5-7 hours, and the nitrogen gas flow rate during the sintering is 60-100 mL / min.
[0020] Preferably, the procedure for heating to the sintering temperature is: first heating to 1200°C at a rate of 4-6°C / min, then heating to 1400°C at a rate of 2-4°C / min, then heating to 1500°C at a rate of 1-3°C / min, and finally heating to the sintering temperature at a rate of 0.5-1.5°C / min.
[0021] The present invention also provides a Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic material prepared by the preparation method described in the above scheme, the chemical formula of which is shown in Formula I:
[0022] Sr 0.01 Lu 0.985 Ti 1-x Ta x O3 formula I;
[0023] In formula I: 0<x≤0.015.
[0024] Preferably, the dielectric constant of the Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material at room temperature and a test frequency of 1 kHz is 156000-253000, and the dielectric loss is 0.02-0.067.
[0025] The present invention provides a method for preparing a SrTiO3-based giant dielectric ceramic material doped with Lu and Ta as donors at the same time, comprising the following steps: (1) ball-milling SrCO3, TiO2, Lu2O3 and Ta2O5 once according to the stoichiometric ratio in formula I (see above), drying the obtained first ball milled material and synthesizing it to obtain a synthetic powder; (2) ball-milling the synthetic powder twice and then sieving and drying it in turn to obtain a secondary ball milled material; (3) mixing the secondary ball milled material, a binder and water, and then aging, granulating and dry pressing it in turn to obtain a ceramic body; (4) debinding and sintering the ceramic body in turn to obtain the SrTiO3-based giant dielectric ceramic material doped with Lu and Ta as donors at the same time; the sintering atmosphere is nitrogen. The present invention utilizes the strontium vacancies generated by Lu and Ta being donor-doped at the A (Sr) position and the B (Ti) position respectively to form a SrTiO3-based giant dielectric ceramic material. Oxygen vacancies and Ti 3+ These defect dipoles tend to form stable defect clusters such as: and These defect clusters will increase the local polarizability to achieve the giant dielectric effect, and will also limit the long-range displacement of free electrons to achieve the purpose of reducing dielectric loss. In addition, the present invention can obtain Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic materials by sintering in a nitrogen atmosphere. The ceramic material has a giant dielectric effect, low dielectric loss, and good frequency and temperature stability of the dielectric constant, which meets the needs of miniaturization of electronic components and energy storage devices for dielectric materials. In addition, the amount of dopants Ta2O5 and Lu2O3 used in the present invention is small, which can reduce production costs; the preparation method involved in the present invention is simple, has good repeatability, high yield, low cost, and is convenient for commercial production.
[0026] The results of the embodiment show that when x=0.01, at room temperature and a test frequency of 1 kHz, the dielectric constant of the SrTiO3-based giant dielectric ceramic material doped with Lu and Ta as donors is ˜220,000 and the dielectric loss is ˜0.02. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 For Sr 0.985 Lu 0.01 Ti 1-x Ta x XRD test results of O3 (x = 0, 0.005, 0.01 and 0.015), where (a) is Sr obtained by sintering at 1525 ° C for 6 h in nitrogen atmosphere. 0.985 Lu 0.01 Ti 1-x Ta xXRD patterns of O3 (x = 0, 0.005, 0.01 and 0.015), (b) is a local enlarged view of the (222) diffraction peak of Lu2Ti2O7, and (c) is a local enlarged view of the (110) diffraction peak of SrTiO3;
[0028] Figure 2 Pure SrTiO3 and Sr 0.985 Lu 0.01 Ti 1-x Ta x Backscattered scanning electron micrographs of O3 and Sr 0.985 Lu 0.01 Ti 1-x Ta x The average grain size and relative density test results of O3, where (a) is a backscattered scanning electron microscope photo of pure SrTiO3, (b) to (e) are surface morphology photos of samples with x = 0, 0.005, 0.01 and 0.015 under a backscattered scanning electron microscope; (f) is a photo of SrTiO3 0.985 Lu 0.01 Ti 1-x Ta x Variation of the average grain size and relative density of O3 with doping concentration;
[0029] Figure 3 Sr was obtained by sintering at 1525℃ for 6h in nitrogen atmosphere. 0.985 Lu 0.01 Ti 1-x Ta x Dielectric properties of O3 ceramics (x = 0, 0.005, 0.01 and 0.015), where (a) is the variation of dielectric properties with frequency at room temperature, (b) is the variation of dielectric properties with doping concentration at room temperature and 1 kHz, and (c) is the variation of dielectric properties with temperature at 1 kHz. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing a Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material, comprising the following steps:
[0031] (1) SrCO3, TiO2, Lu2O3 and Ta2O5 are ball-milled once according to the stoichiometric ratio in formula I, and the ball-milled material obtained is dried and then synthesized to obtain a synthetic powder;
[0032] Sr 0.01 Lu 0.985 Ti 1-x Ta x O3 formula I;
[0033] In formula I: 0<x≤0.015;
[0034] (2) ball-milling the synthetic powder for a second time, followed by sieving and drying in sequence to obtain a second ball-milled material;
[0035] (3) mixing the secondary ball mill material, a binder and water, and then performing aging, granulation and dry pressing in sequence to obtain a ceramic body;
[0036] (4) Debinding and sintering the ceramic body in sequence to obtain the Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material; the sintering atmosphere is nitrogen.
[0037] According to the stoichiometric ratio in formula I, SrCO3, TiO2, Lu2O3 and Ta2O5 are ball-milled once, and the ball-milled material is dried and synthesized to obtain a synthetic powder. In the present invention, the value of x in formula I is preferably 0.005, 0.01 or 0.015, and more preferably 0.01. In the present invention, the purity of the SrCO3 is preferably above 99%, the purity of the TiO2 is preferably above 99%, the purity of the Lu2O3 is preferably above 99.99%, and the purity of the Ta2O5 is preferably above 99.99%; the conditions for the primary ball milling preferably include: a ball milling speed of 250 to 350 rpm, more preferably 280 to 300 rpm, a ball milling time of 5 to 7 h, more preferably 5.5 to 6.5 h, and a ball milling medium of deionized water; the ball milling device is preferably a planetary ball mill, and the ball milling jar used for the ball milling is preferably a polytetrafluoroethylene ball milling jar; the present invention has no special requirements for the drying conditions, and drying in an oven is sufficient.
[0038] In the present invention, the synthesis temperature is preferably 1150-1250°C, more preferably 1200°C, the synthesis holding time is preferably 3-5h, more preferably 4h; the heating rate to the synthesis temperature is preferably 4-6°C / min, more preferably 5°C / min. In a specific embodiment of the present invention, the dried primary ball mill is preferably placed in an alumina crucible and then synthesized in a muffle furnace.
[0039] After obtaining the synthetic powder, the present invention performs secondary ball milling on the synthetic powder, and then sieves and dries in sequence to obtain secondary ball milled material. In the present invention, the conditions for the secondary ball milling preferably include: a ball milling speed of 250 to 350 rpm, more preferably 280 to 300 rpm, a ball milling time of 5 to 7 hours, more preferably 5.5 to 6.5 hours, and a ball milling medium of deionized water; the mesh number of the sieve for sieving is preferably 500 meshes; the present invention has no special requirements for the drying conditions, and drying in an oven is sufficient.
[0040] After obtaining the secondary ball mill, the present invention mixes the secondary ball mill, a binder and water, and then performs aging, granulation and dry pressing in sequence to obtain a ceramic body. In the present invention, the binder is preferably a polyvinyl alcohol solution, specifically a polyvinyl alcohol aqueous solution; the mass concentration of the polyvinyl alcohol solution is preferably 3-5%, more preferably 4%; the amount of the binder is preferably 1-2% of the mass of the synthetic powder, more preferably 1.5-2%, and the amount of water is preferably 0.5-1% of the mass of the synthetic powder; the water is preferably deionized water; the aging time is preferably 8-24h, more preferably 12-20h; the present invention has no special requirements for the granulation, and the conditions well known in the art can be used; the pressure of the dry pressing is preferably 13-17MPa, more preferably 15MPa; the diameter of the ceramic body is preferably 8-12mm, more preferably 10mm, and the thickness is preferably 1-2mm.
[0041] After obtaining the ceramic body, the present invention sequentially debinds and sinters the ceramic body to obtain the Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic material; the sintering is performed in a nitrogen atmosphere. In the present invention, the debinding temperature is preferably 550-650°C, more preferably 600°C, the debinding holding time is preferably 1.5-2.5h, more preferably 2h; the debinding is preferably performed in a muffle furnace.
[0042] In the present invention, the sintering temperature is preferably 1500-1550°C, more preferably 1525°C, the sintering holding time is preferably 5-7h, more preferably 5.5-6.5h, and further preferably 6h; the procedure for heating to the sintering temperature is preferably: first heating to 1200°C at a rate of 4-6°C / min, then heating to 1400°C at a rate of 2-4°C / min, then heating to 1500°C at a rate of 1-3°C / min, and finally heating to the sintering temperature at 0.5-1.5°C / min; the sintering is preferably carried out in a tubular furnace.
[0043] The present invention also provides a Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic material prepared by the preparation method described in the above scheme, the chemical formula of which is shown in Formula I:
[0044] Sr 0.01 Lu 0.985 Ti 1-x Ta x O3 formula I;
[0045] In formula I: 0<x≤0.015.
[0046] In the present invention, x in Formula I is preferably 0.005, 0.01 or 0.015.
[0047] In the present invention, the dielectric constant of the Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic material at room temperature and a test frequency of 1 kHz is 156000-253000, and the dielectric loss is 0.02-0.067.
[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] Step 1: Using SrCO3 (purity 99%), TiO2 (purity 99%), Ta2O5 (purity 99.99%) and Lu2O3 (purity 99.99%) as starting materials, according to the chemical formula Sr 0.01 Lu 0.985 Ti 1-x Ta x O3 (x = 0) weigh the raw materials, the total mass of the raw materials is 30g, add the weighed raw materials into a polytetrafluoroethylene ball mill, use deionized water as the ball milling medium, mix and ball mill for 8h at a speed of 300rpm on a planetary ball mill, and then put them into an oven for drying.
[0051] Step 2: The powder dried in step 1 is loaded into an alumina crucible, heated to 1200°C in a muffle furnace at a heating rate of 5°C / min and kept warm for 4 hours to obtain synthetic powder, and then secondary ball milling is performed using the same process as step 1, and the powder is sieved through a 500-mesh sieve and dried to obtain secondary ball milling material.
[0052] Step 3: Add 0.5 g of 4 wt% PVA solution and 0.2 g of deionized water to the secondary ball mill obtained in step 2, and perform aging, granulation, and dry pressing in sequence. The dry pressing pressure is 15 MPa, and the ceramic body obtained by molding has a diameter of 10 mm and a thickness of 2 mm.
[0053] Step 4: Place the ceramic body obtained in step 3 in a muffle furnace and heat it to 600°C and keep it for 2 hours to remove the binder. Then place it in a tubular furnace and heat it to 1200°C at a nitrogen flow rate of 80 mL / min at a heating rate of 5°C / min. Then heat it to 1400°C at 3°C / min, heat it to 1500°C at 2°C / min, and finally heat it to 1525°C at 1°C / min and keep it for 6 hours. The sintering process is performed to obtain Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic materials.
[0054] The ceramic sheet obtained by sintering was polished on both sides and coated with silver electrodes, and then placed in a muffle furnace and heated to 550°C for 15 minutes to sinter the electrodes. The dielectric properties were tested using an Agilent 4294A impedance analyzer. The test results showed that the dielectric constant of the ceramic material was ~216000 and the dielectric loss was ~0.067 at room temperature and a test frequency of 1kHz.
[0055] Example 2
[0056] Step 1: SrCO3 (purity 99%), TiO2 (purity 99%), Ta2O5 (purity 99.99%) and Lu2O3 (purity 99.99%) were prepared according to the chemical formula Sr 0.01 Lu 0.985 Ti 1-x Ta x O3 (x = 0.005) weighed raw materials, the total mass of the raw materials was 30g, the weighed raw materials were added into a polytetrafluoroethylene ball mill, deionized water was used as the ball milling medium, mixed and ball milled on a planetary ball mill at a speed of 300rpm for 8h, and then put into an oven for drying.
[0057] Step 2: The powder dried in step 1 is loaded into an alumina crucible, heated to 1200°C in a muffle furnace at a heating rate of 5°C / min and kept warm for 4 hours to obtain synthetic powder, and secondary ball milling is performed using the same process as step 1, and the powder is sieved through a 500-mesh sieve and then dried to obtain secondary ball milling material.
[0058] Step 3: Add 0.5 g of 4 wt% PVA solution and 0.2 g of deionized water to the secondary ball mill obtained in step 2, and perform aging, granulation, and dry pressing in sequence. The dry pressing pressure is 15 MPa, and the ceramic body obtained by molding has a diameter of 10 mm and a thickness of 2 mm.
[0059] Step 4: Place the ceramic body obtained in step 3 in a muffle furnace and heat it to 600°C and keep it for 2 hours to remove the binder. Then place it in a tubular furnace and heat it to 1200°C at a nitrogen flow rate of 80 mL / min at a heating rate of 5°C / min. Then heat it to 1400°C at 3°C / min, heat it to 1500°C at 2°C / min, and finally heat it to 1525°C at 1°C / min and keep it for 6 hours. The sintering process is performed to obtain Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic materials.
[0060] The ceramic sheet obtained by sintering was polished on both sides and coated with silver electrodes, and then placed in a muffle furnace and heated to 550°C for 15 minutes to sinter the electrodes. The dielectric properties were tested using an Agilent 4294A impedance analyzer. The test results showed that the dielectric constant of the ceramic material was ~156000 and the dielectric loss was ~0.029 at room temperature and a test frequency of 1kHz.
[0061] Example 3
[0062] Step 1: SrCO3 (purity 99%), TiO2 (purity 99%), Ta2O5 (purity 99.99%) and Lu2O3 (purity 99.99%) were prepared according to the chemical formula Sr 0.01 Lu 0.985 Ti 1-x Ta x O3 (x = 0.01) weigh the raw materials, the total mass of the raw materials is 30g, add the weighed raw materials into a polytetrafluoroethylene ball mill, use deionized water as the ball milling medium, mix and ball mill for 8h at a speed of 300rpm on a planetary ball mill, and then put it into an oven for drying.
[0063] Step 2: The powder dried in step 1 is loaded into an alumina crucible, heated to 1200°C in a muffle furnace at a heating rate of 5°C / min and kept warm for 4 hours to obtain synthetic powder, and then secondary ball milling is performed using the same process as step 1, and the powder is sieved through a 500-mesh sieve and dried to obtain secondary ball milling material.
[0064] Step 3: Add 0.5 g of 4 wt% PVA solution and 0.2 g of deionized water to the secondary ball mill obtained in step 2, and perform aging, granulation, and dry pressing in sequence. The dry pressing pressure is 15 MPa, and the ceramic body obtained by molding has a diameter of 10 mm and a thickness of 2 mm.
[0065] Step 4: Place the ceramic body obtained in step 3 in a muffle furnace and heat it to 600°C for 2 hours to remove binder. Then place it in a tubular furnace and heat it to 1200°C at a nitrogen flow rate of 80mL / min at a heating rate of 5°C / min, then heat it to 1400°C at 3°C / min, then heat it to 1500°C at 2°C / min, and finally heat it to 1525°C at 1°C / min and keep it for 6 hours to obtain Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic materials.
[0066] The ceramic sheet obtained by sintering was polished on both sides and coated with silver electrodes, and then placed in a muffle furnace and heated to 550°C for 15 minutes to sinter the electrodes. The dielectric properties were tested using an Agilent 4294A impedance analyzer. The test results showed that the dielectric constant of the ceramic material was ~220,000 and the dielectric loss was ~0.02 at room temperature and a test frequency of 1kHz.
[0067] Example 4
[0068] Step 1: SrCO3 (purity 99%), TiO2 (purity 99%), Ta2O5 (purity 99.99%) and Lu2O3 (purity 99.99%) were prepared according to the chemical formula Sr 0.01 Lu 0.985 Ti 1-x Tax O3 (x = 0.015) weighed raw materials, the total mass of the raw materials was 30g, the weighed raw materials were added into a polytetrafluoroethylene ball mill, deionized water was used as the ball milling medium, mixed and ball milled on a planetary ball mill at a speed of 300rpm for 8h, and then put into an oven for drying.
[0069] Step 2: The powder dried in step 1 is loaded into an alumina crucible, heated to 1200°C at a heating rate of 5°C / min in a muffle furnace and kept warm for 4 hours to synthesize powder, and then ball-milled for the second time using the same process as step 1, sieved through a 500-mesh sieve, and dried to obtain a secondary ball-milled material.
[0070] Step 3: Add 0.5 g of 4 wt% PVA solution and 0.2 g of deionized water to the secondary ball mill obtained in step 2, and perform aging, granulation, and dry pressing in sequence. The dry pressing pressure is 15 MPa, and the ceramic body obtained by molding has a diameter of 10 mm and a thickness of 2 mm.
[0071] Step 4: Place the ceramic body obtained in step 3 in a muffle furnace and heat it to 600°C and keep it for 2 hours to remove the binder. Then place it in a tubular furnace and heat it to 1200°C at a nitrogen flow rate of 80 mL / min at a heating rate of 5°C / min. Then heat it to 1400°C at 3°C / min, heat it to 1500°C at 2°C / min, and finally heat it to 1525°C at 1°C / min and keep it for 6 hours. The sintering process is performed to obtain Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic materials.
[0072] The ceramic sheet obtained by sintering was polished on both sides and coated with silver electrodes, and then placed in a muffle furnace and heated to 550°C for 15 minutes to sinter the electrodes. The dielectric properties were tested using an Agilent 4294A impedance analyzer. The test results showed that the dielectric constant of the ceramic material was ~253000 and the dielectric loss was ~0.03 at room temperature and a test frequency of 1kHz.
[0073] Testing and Characterization
[0074] Testing and characterization of ceramic materials obtained in Examples 1 to 4
[0075] (1) XRD test
[0076] Figure 1 For Sr 0.985 Lu 0.01 Ti 1-x Ta x XRD test results of O3 (x = 0, 0.005, 0.01 and 0.015), where (a) is Sr obtained by sintering at 1525 ° C for 6 h in nitrogen atmosphere. 0.985 Lu 0.01 Ti 1-x Ta xO3 (x = 0, 0.005, 0.01 and 0.015), (b) is a local enlarged view of the (222) diffraction peak of Lu2Ti2O7, and (c) is a local enlarged view of the (110) diffraction peak of SrTiO3. Figure 1 As can be seen from (a) in Figure 1, the main crystalline phase of all samples presents a cubic perovskite structure and corresponds well to PDF#84-0444. A small amount of the second phase Lu2Ti2O7 corresponding to PDF#76-1696 can be detected in all samples with x=0 to 0.015. The local enlarged image of the (222) diffraction peak of Lu2Ti2O7 is shown in Figure 1. Figure 1 As shown in (b) in Figure 2, we can see that as Ta 5+ The intensity of the (222) diffraction peak of Lu2Ti2O7 gradually increases with the increase of doping concentration, which indicates that Ta 5+ The doping of will compete with Lu for lattice positions at Ti positions, promoting the precipitation of the second phase Lu2Ti2O7. In addition, with the increase of doping concentration, the diffraction peak of Lu2Ti2O7 gradually shifts to a lower angle, which indicates an increase in the unit cell parameters. This may be due to the fact that a small number of ions have a larger radius. Solid solution into the Lu2Ti2O7 lattice causes lattice expansion. Figure 1 As can be seen in (c), compared with pure SrTiO3, the diffraction peak of the sample with x = 0 shifts to a higher angle, which is due to the smaller ionic radius. Sr dissolved in SrTiO3 2+ The unit cell parameters are reduced. 5+ As the doping amount increases, the diffraction peak gradually shifts to a lower angle, and the unit cell parameter increases to x = 0.015. This is due to the larger ionic radius of Ta 5+ Ti dissolved in SrTiO3 4+ The site causes an increase in the unit cell parameters.
[0077] (2) Backscattered scanning electron microscopy and average grain size test
[0078] Figure 2 (a) to (e) show pure SrTiO3 and Ta 5+ Surface morphology of samples with doping concentrations of x = 0, 0.005, 0.01 and 0.015 under backscattered scanning electron microscope. The bright white particles found at the grain boundaries of samples with x = 0, 0.005, 0.01 and 0.015 are the second phase Lu2Ti2O7. The average grain size was calculated using Nanomeasure software. Figure 2(f) is a graph showing the variation of average grain size with doping concentration. Compared with pure SrTiO3, the average grain size of the x=0 sample increases sharply from 2.09 μm to 19.59 μm, which is mainly due to the Lu 3+ However, as Ta 5+ As the doping amount of Ta increases, the grain size gradually decreases to 5.91μm when x=0.015. The reduction in grain size is related to the pinning effect of the second phase. Ta doping helps the second phase to precipitate and enhance its pinning effect. Therefore, despite the increasing defect concentration, the average grain size remains at around 6μm as the content of the second phase Lu2Ti2O7 increases. Figure 2 (f) in the figure also shows the variation of relative density with doping concentration. It can be found that the relative density of the ceramic material is the largest at x=0, which is 97.32%, and then decreases slightly, which may be related to the change of its grain size.
[0079] (3) Dielectric properties test
[0080] Figure 3 The Sr sintered at 1525℃ for 6h in nitrogen atmosphere is shown. 0.985 Lu 0.01 Ti 1-x Ta x Dielectric properties of O3 ceramics (x = 0, 0.005, 0.01 and 0.015). Figure 3 (a) shows the variation of dielectric properties with frequency at room temperature. All Sr sintered in N2 0.985 Lu 0.01 Ti 1-x Ta x The O3 ceramics all show similar dielectric responses, with a slight decrease in the dielectric constant at higher frequencies, which may be related to the interface polarization because the interface polarization does not respond at high frequencies. Figure 3 (b) shows the change of dielectric properties with doping concentration at room temperature and 1kHz. It can be found that compared with pure SrTiO3, single element doping of Lu (x = 0) will make the dielectric constant (ε r ) increases to ~216000, and the dielectric loss (tanδ) increases to ~0.067. As the doping amount of Ta increases, the dielectric constant and dielectric loss show a trend of first decreasing and then increasing. The best dielectric performance is obtained when x=0.01, and the dielectric constant is ε r ~220000, and the dielectric loss is tanδ~0.02. Combined with the above XPS defect analysis, it can be seen that the improvement of dielectric properties is closely related to the defect concentration. Figure 3 (c) shows the change of dielectric properties with temperature at 1kHz. It can be found that Ta 5+The temperature stability of dielectric loss of doped samples has been significantly improved, which may be related to the increase in defect concentration.
[0081] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material, characterized in that: The following steps are involved: (1) SrCO3, TiO2, Lu2O3 and Ta2O5 are ball-milled once according to the stoichiometric ratio in formula I, and the ball-milled material obtained is dried and then synthesized to obtain a synthetic powder; Sr 0.01 Lu 0.985 Ti 1-x The x O3 formula I; In formula I: 0<x≤0.015; (2) ball-milling the synthetic powder for a second time, followed by sieving and drying in sequence to obtain a second ball-milled material; (3) mixing the secondary ball mill material, a binder and water, and then performing aging, granulation and dry pressing in sequence to obtain a ceramic body; (4) Debinding and sintering the ceramic body in sequence to obtain the Lu and Ta simultaneously donor-doped SrTiO3-based giant dielectric ceramic material; the sintering atmosphere is nitrogen.
2. The preparation method according to claim 1, characterized in that: The conditions of the primary ball milling and the secondary ball milling independently include: the ball milling speed is 250-350 rpm, the ball milling time is 5-7 hours, and the ball milling medium is deionized water.
3. The preparation method according to claim 1, characterized in that: The synthesis temperature is 1150-1250° C., and the heat preservation time is 3-5 hours; the heating rate to the synthesis temperature is 4-6° C. / min; and the synthesis atmosphere is air.
4. The preparation method according to claim 1, characterized in that: The binder is a polyvinyl alcohol solution, the concentration of which is 3-5 wt. %; the amount of the binder is 1-2 % of the mass of the synthetic powder; and the amount of water is 0.5-1 % of the mass of the synthetic powder.
5. The preparation method according to claim 1, characterized in that: The dry pressing pressure is 13-17 MPa; the diameter of the ceramic body is 8-12 mm, and the thickness is 1-2 mm.
6. The preparation method according to claim 1, characterized in that: The debinding temperature is 550-650° C., and the heat preservation time is 1.5-2.5 hours.
7. The preparation method according to claim 1, characterized in that: The sintering temperature is 1500-1550° C., the heat preservation time is 5-7 hours, and the nitrogen gas flow rate during the sintering is 60-100 mL / min.
8. The preparation method according to claim 1 or 7, characterized in that: The procedure for heating to the sintering temperature is: first heating to 1200°C at a rate of 4-6°C / min, then heating to 1400°C at a rate of 2-4°C / min, then heating to 1500°C at a rate of 1-3°C / min, and finally heating to the sintering temperature at a rate of 0.5-1.5°C / min.
9. The Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic material prepared by the preparation method according to any one of claims 1 to 7 has a chemical formula as shown in Formula I: Sr 0.01 Lu 0.985 Ti 1-x The x O3 formula I; In formula I: 0<x≤0.
015.
10. The Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic material according to claim 9, characterized in that: The dielectric constant of the Lu and Ta donor-doped SrTiO3-based giant dielectric ceramic material at room temperature and a test frequency of 1 kHz is 156000-253000, and the dielectric loss is 0.02-0.067.
Citation Information
Patent Citations
Dielectric ceramic material with giant dielectric constant and low dielectric loss and method for preparing dielectric ceramic material
CN105777111A
Complex-phase giant dielectric ceramic material with high breakdown field strength and preparation method thereof
CN113831121A
Lu-doped strontium titanate-based giant dielectric ceramic material and preparation method thereof
CN116854463A
Ta and Al co-doped strontium titanate-based giant dielectric ceramic material and preparation method thereof
CN117401970A
A-site and B-site double-donor co-doped strontium titanate-based giant dielectric ceramic material and preparation method thereof
CN118530019A