Method for synergistically preparing ceramsite from arsenic alkali leaching residues and fly ash

Through the ignition smelting collaborative roasting technology, the arsenic alkali leaching slag and fly ash are prepared, which solves the problems of recovery of arsenic and antimony components and fixes alkaline components, and realizes the efficient resource utilization and environmental protection of the ceratops. Building materials performance requirements.

CN118930305APending Publication Date: 2024-11-12CENT SOUTH UNIV

Patent Information

Application Number
CN202411150891.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively resource and circulate the arsenic alkali leaching slag, resulting in waste of antimony and alkali resources and environmental pollution, and fly ash has failed to be safely disposed of, affecting the environment and human health.

Method used

Through the ignition smelting and co-roasting technology, the arsenic alkali leaching slag and fly ash are dried ball milled, and mixed with silica, binder and carbonaceous reducing agent, and ball-making and drying through a disc ball making machine. and roasting to form porous ceramic granules, realize the volatile recovery of arsenic and antimony components and the fixation of alkaline components, and use components such as SiO2, Al2O3 and Fe2O3 in fly ash to build the ceramic granule framework.

Benefits of technology

The recovery of arsenic antimony components and the fixation of alkaline components are achieved, and the excellent performance of ceramic granules are prepared to meet the requirements of building materials, improve resource utilization, and reduce environmental pollution risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003630080000041
    Figure BDA0005003630080000041
  • Figure BDA0005003630080000042
    Figure BDA0005003630080000042
  • Figure BDA0005003630080000051
    Figure BDA0005003630080000051
Patent Text Reader

Abstract

The invention discloses a method for synergistically preparing ceramsite from arsenic alkali leaching residues and fly ash, and belongs to the technical field of solid waste treatment. Carrying out dry ball milling treatment on the arsenic alkali leaching residues and fly ash, and pelletizing with silicon dioxide, a binder, a carbonaceous reducing agent and water through a disc pelletizer to obtain a ceramsite raw material; the ceramsite raw material is dried and roasted to obtain ceramsite; according to the method, through the pyrometallurgy and roasting technology, harmful elements such as arsenic and antimony in the arsenic-alkali leaching residues are volatilized and recycled, residual alkali components are fully utilized and fixed, meanwhile, SiO2, Al2O3 and Fe2O3 components in the fly ash are recycled, and the obtained ceramsite product is excellent in performance and meets the application requirements of building materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for resource disposal of arsenic alkali leaching residue and fly ash, and in particular to a method for collaboratively preparing ceramsite from arsenic alkali leaching residue and fly ash, belonging to the technical field of solid waste disposal. Background Art

[0002] Arsenic-alkali leaching slag is the filtered slag after wet arsenic removal from the arsenic-alkali slag produced during the antimony smelting process. It contains insoluble arsenic-antimony components and a large amount of alkaline components. If not treated, it will have a huge impact on the ecological environment. At present, due to the technical bottlenecks of low resource utilization rate, limited product market, high disposal cost, and secondary pollution risk in the treatment of arsenic-alkali slag, most of the large amount of arsenic-alkali slag produced by antimony-related enterprises has long been disposed of by direct flexible landfill, resulting in a large amount of antimony and alkali resources waste and certain environmental problems.

[0003] Fly ash is the fly ash produced when coal is burned at high temperature. If it is not safely disposed of as a resource, it will cause great harm to the environment and human life. Fly ash is mainly composed of metal oxides such as SiO2, Al2O3, Fe2O3, CaO, etc. The rational use of fly ash is of great significance for resource development. It plays an important role in the construction industry, soil modification, zeolite preparation, etc.

[0004] The use of solid waste to prepare high-quality ceramsite is conducive to the disposal of solid waste and the recycling of minerals. As a building material, ceramsite has excellent physical properties and environmental protection characteristics. Fly ash contains abundant SiO2, Al2O3 and Fe2O3 components, which are the raw material components required for the preparation of ceramsite. It has been used to prepare ceramsite. For example, Chinese patent CN104418581A discloses a fly ash processing process, which is specifically: a. Mix and stir the dried fly ash, the clay that is ball-milled after drying, and the coal that is ball-milled, and the ratio of fly ash, clay and coal is 70-80%, 5-10% and 10-20% respectively; b. Ball processing; c. Sintering; d. Crushing and screening. The prepared fly ash ceramsite has good thermal insulation, good fire resistance, good seismic performance, low water absorption, good antifreeze performance and durability. However, due to the high content of harmful elements such as arsenic and antimony in arsenic-alkali leaching residue and its high sodium characteristics, it is difficult to consume it as a building material. At present, there are few reports on the use of arsenic-alkali leaching residue to prepare expanded clay. Summary of the invention

[0005] In view of the fact that the existing technical means are difficult to resource and efficiently recycle the arsenic alkali leaching residue, the purpose of the present invention is to provide a method for preparing ceramsite by coordinating the arsenic alkali leaching residue and fly ash. The method uses the pyrometallurgical smelting and co-roasting technology to not only realize the volatilization and recovery of harmful elements such as arsenic and antimony in the arsenic alkali leaching residue, but also fully utilize and fix the residual alkali component, while realizing the resource utilization of components such as SiO2, Al2O3 and Fe2O3 in the fly ash. The obtained ceramsite product has excellent performance and meets the application requirements of building materials.

[0006] In order to achieve the above technical purpose, the present invention provides a method for preparing ceramsite by arsenic alkali leaching residue and fly ash. The method comprises the following steps: subjecting the arsenic alkali leaching residue and fly ash to dry ball milling, and then pelletizing the pellets with silicon dioxide, a binder, a carbonaceous reducing agent and water through a disc pelletizing machine to obtain ceramsite raw material; and the ceramsite raw material is dried and roasted to obtain ceramsite.

[0007] The technical solution of the present invention uses arsenic alkali leaching slag and fly ash as the main raw materials to prepare ceramsite, which is mainly based on the chemical composition characteristics of arsenic alkali leaching slag and fly ash itself. For example, arsenic alkali leaching slag contains a large amount of alkaline components and components such as SiO2, Al2O3, and fly ash contains components such as SiO2, Al2O3 and Fe2O3. The two are matched and these components can form a ceramsite skeleton structure with excellent physical and chemical properties through high-temperature solid-phase reaction. The insoluble arsenic antimony component and alkali component contained in the arsenic alkali slag are harmful components, and the present invention cleverly introduces a carbonaceous reducing agent, recovers the arsenic antimony component by volatilization during the high-temperature roasting process, and uses the gasification volatilization process of the arsenic antimony component to form pores inside the ceramsite, thereby forming a porous ceramsite structure, and the remaining alkaline components react chemically with components such as SiO2, Al2O3 and Fe2O3 during the roasting process to form a ceramsite skeleton structure to achieve the fixation of alkaline substances. In summary, the present invention realizes the volatilization recovery of arsenic and antimony components in arsenic alkali leaching residue, the fixation of alkaline components, and the full utilization of silicon and aluminum components, and obtains ceramsite with good comprehensive performance, truly realizing the resource utilization of arsenic alkali leaching residue.

[0008] As a preferred solution, the mass ratio of the arsenic alkali leaching residue to the fly ash is 4 to 6: 1. The arsenic alkali leaching residue mainly provides SiO2 and Na2O components, while the fly ash mainly provides SiO2, Al2O3 and Fe2O3 components. The combination of the two in an appropriate proportion is conducive to obtaining a ceramic phase with high mechanical strength. For example, if the proportion of arsenic alkali leaching residue is too high, a glass phase is easily formed, thereby reducing the mechanical strength.

[0009] As a preferred solution, the arsenic alkali leaching residue and the fly ash are ball-milled to a particle size of less than 50 meshes. The ball-milling process uses a dry ball mill to ball-mill to an appropriate particle size, which is beneficial to the subsequent granulation process and high-temperature solid-phase reaction process.

[0010] As a preferred solution, the amount of silicon dioxide used is to adjust the silicon-aluminum mass ratio in the system to 5:1 to 8:1. By controlling the appropriate silicon-aluminum ratio, the ceramsite skeleton can be ensured to have a higher mechanical strength. The amount of silicon dioxide used is to adjust the silicon-aluminum mass ratio in the system to further 5:1 to 7:1.

[0011] As a preferred solution, the amount of the carbonaceous reducing agent is 5% to 8% of the total mass of the arsenic alkali leaching residue and the fly ash. The amount of the carbonaceous reducing agent mainly depends on the content of arsenic and antimony components in the arsenic alkali leaching residue and the fly ash. The carbonaceous reducing agent mainly reduces and volatilizes the arsenic and antimony components. As a more preferred solution, the carbonaceous reducing agent includes at least one of activated carbon and coal.

[0012] As a preferred solution, the amount of the binder is 3-7% of the total mass of the ceramsite raw material. As a more preferred solution, the binder includes at least one of bentonite, aluminum dihydrogen phosphate, and water glass. These binders are common pellet binders in the prior art.

[0013] As a preferred solution, the particle size of the ceramsite raw material is controlled between 5 and 25 mm. The particle size of the ceramsite raw material is further preferably controlled between 10 and 20 mm. The particle size of the ceramsite raw material affects the roasting effect. If the particle size is too large or too small, it is not suitable to obtain ceramsite with good comprehensive performance.

[0014] As a preferred solution, the drying conditions are: temperature of 100-110° C. and time of 1.5-2.0 h.

[0015] As a preferred solution, the roasting conditions are as follows: the roasting temperature is 800-1000°C, the heating rate is 5-15°C / min, and the time is 30min-60min. During the roasting process of ceramsite raw balls, the arsenic and antimony components in the arsenic alkali leaching slag are removed in the form of volatiles, and the pores inside the ceramsite are formed at the same time. The silicon, aluminum and other components in the fly ash react with the alkaline components in the arsenic alkali leaching slag to form the skeleton structure of the ceramsite. The roasting is carried out in a rotary atmosphere furnace. The roasting conditions mainly affect the performance of the ceramsite and the arsenic and antimony recovery rate. If the roasting temperature is lower and the time is shorter, the reduction and volatilization effect of arsenic and antimony is lower, and the strength of the ceramsite formed by sintering is lower. If the roasting temperature is too high or the roasting time is too long, dense sintering will occur, reducing the porosity of the ceramsite and increasing its apparent density.

[0016] Compared with the existing technical means for treating arsenic alkali leaching residue, the technical solution of the present invention has the following beneficial technical effects:

[0017] 1. The present invention effectively removes arsenic and antimony components in arsenic alkali leaching slag through a pyrometallurgical coordinated roasting method, and simultaneously utilizes the alkali component to participate in a chemical reaction to form a ceramsite skeleton to achieve alkali fixation, thereby achieving its safe disposal and avoiding environmental pollution.

[0018] 2. The present invention makes full use of silicon, aluminum and other components in fly ash to react with the alkali components and silicon and aluminum components in arsenic alkali leaching residue to construct a ceramsite skeleton, and uses the components contained in the ceramsite to achieve pore formation, thereby preparing a ceramsite product with excellent performance and improving resource utilization.

[0019] 3. The method of the present invention is easy to operate, does not require complicated equipment and process conditions, has low cost, and is easy for industrial production. DETAILED DESCRIPTION

[0020] The following specific examples are intended to further illustrate the present invention rather than to limit the scope of protection of the claims.

[0021] The arsenic alkali leaching residue from Lengshuijiang Xikuangshan and Liupanshui fly ash were used as the experimental research objects. The following table 1 shows the main element composition of the arsenic alkali leaching residue, and the following table 2 shows the main element composition of the fly ash. The element composition of the arsenic alkali leaching residue is complex, mainly composed of sodium, aluminum, silicon, antimony and other elements, of which the silicon content is 12.12%, the sodium content is 21.61%, the antimony content is 3.406%, and the arsenic content is 2.650%. The elements in fly ash are complex, mainly composed of calcium, aluminum, silicon, iron and other elements, of which the silicon content is 21.079%, the aluminum content is 8.567%, the calcium content is 6.834%, and the iron content is 4.142%.

[0022] Table 1 Main element composition of arsenic alkali leaching residue

[0023]

[0024] Table 2 Main element composition of fly ash

[0025]

[0026] Example 1

[0027] The arsenic alkali leaching slag and fly ash are crushed and ground to a particle size of less than -50 mesh, and 500g of the arsenic alkali leaching slag after crushing and grinding is weighed. The arsenic alkali leaching slag and fly ash are mixed with SiO2, a binder, and a reducing agent in a certain proportion. The amount of fly ash is controlled at a ratio of 4:1, 5:1, and 6:1 between the arsenic alkali leaching slag and the fly ash. The binder is bentonite, and its mass percentage content is 10% of the total mass; the reducing agent is activated carbon, and its amount is 5% of the total slag; the amount of added quartz powder should be controlled at a ratio of silicon to aluminum of 6:1. After the materials are fully mixed, add 25% of the total mass of water to the mixture, and mix it evenly through stirring or agitator and other equipment to ensure that the materials form a mixture with good viscosity and plasticity. Use a disc ball making machine to ball the mixture, control the raw ball particle size to be about 15mm, and form uniform ceramsite raw balls. After forming, the spheres are placed in an oven for thorough drying. The oven temperature is set at 105°C and the drying time is not less than 1.5 hours, until the moisture content of the raw balls is less than 3%. During the pyrometallurgical process, a small rotary atmosphere furnace is charged with argon gas, and the temperature is raised from room temperature to the set temperature at a rate of 10°C / min. The roasting temperature is set to 900°C. The roasting time is controlled to 45 minutes to ensure that the material reacts fully. After roasting, the furnace is cooled and the ceramsite temperature is taken out after it drops below 500°C, completing the preparation of the ceramsite and realizing resource recycling and environmental protection. The specific data are shown in Table 3 below.

[0028] Table 3 Effect of the ratio of arsenic alkali leaching residue and fly ash on the performance of ceramsite

[0029]

[0030] Example 2

[0031] The arsenic alkali leaching slag and fly ash are crushed and ground to a particle size of less than -50 mesh. 500g of arsenic alkali leaching slag and 100g of fly ash are weighed after the crushing and grinding. The arsenic alkali leaching slag and fly ash are mixed with SiO2, a binder, and a reducing agent in a certain proportion. The binder is bentonite, and its mass percentage content is 10% of the total mass; the reducing agent is activated carbon, and its amount is 5% of the total slag; the amount of added quartz powder should be controlled to be 5:1, 6:1, 7:1, 8:1 in the ratio of silicon to aluminum. After the materials are fully mixed, add 25% of the total mass of water to the mixture, and mix it evenly through stirring or agitator and other equipment to ensure that the materials form a mixture with good viscosity and plasticity. Use a disc ball making machine to ball the mixture, control the raw ball particle size to be about 15mm, and form a uniform ceramsite raw ball. After forming, the spheres are placed in an oven for thorough drying. The oven temperature is set at 105°C and the drying time is not less than 1.5 hours, until the moisture content of the raw balls is less than 3%. During the pyrometallurgical process, a small rotary atmosphere furnace is charged with argon gas, and the temperature is raised from room temperature to the set temperature at a rate of 10°C / min. The roasting temperature is set to 900°C. The roasting time is controlled to 45 minutes to ensure that the material reacts fully. After roasting, the furnace is cooled and the ceramsite temperature is taken out after it drops below 500°C, completing the preparation of the ceramsite and realizing resource recycling and environmental protection. The specific data are shown in Table 4 below.

[0032] Table 4 Effect of silicon-aluminum ratio on ceramsite performance

[0033]

[0034] Example 3

[0035] The arsenic alkali leaching slag and fly ash are crushed and ground to a particle size of less than -50 mesh. 500g of arsenic alkali leaching slag and 100g of fly ash are weighed after the crushing and grinding. The arsenic alkali leaching slag and fly ash are mixed with SiO2, binder and reducing agent in a certain proportion. The binder is bentonite, and its mass percentage content is 10% of the total mass; the reducing agent is activated carbon, and its amount is 5% of the total slag; the amount of added quartz powder is controlled to be 6:1 in the ratio of silicon to aluminum. After the materials are fully mixed, add water with a total amount of 25% of the total mass of the raw materials to the mixture, and mix it evenly through stirring or agitator and other equipment to ensure that the materials form a mixture with good viscosity and plasticity. The mixed material is balled using a disc ball making machine, and the particle size of the raw ball is controlled to be about 15mm to form a uniform ceramsite raw ball. After the molding is completed, the spheres are placed in an oven for full drying. The oven is set at a temperature of 105°C and the drying time is not less than 1.5 hours until the moisture content of the raw ball is less than 3%. During the pyrometallurgical process, a small rotary atmosphere furnace is charged with argon gas, and the temperature is raised from room temperature to the set temperature at 10°C / min. The roasting temperatures are set to 800°C, 900°C and 1000°C respectively. The roasting time is controlled to 45 minutes to ensure that the materials react fully. After the roasting is completed, the furnace is cooled and the ceramsite temperature is taken out after it drops below 500°C, completing the preparation of ceramsite and realizing resource recycling and environmental protection. The specific data are shown in Table 5 below.

[0036] Table 5 Effect of calcination temperature on the properties of ceramsite

[0037]

[0038]

[0039] Example 4

[0040] The arsenic alkali leaching slag and fly ash are crushed and ground to a particle size of less than -50 mesh. 500g of arsenic alkali leaching slag and 100g of fly ash are weighed after the crushing and grinding. The arsenic alkali leaching slag and fly ash are mixed with SiO2, binder and reducing agent in a certain proportion. The binder is bentonite, and its mass percentage content is 10% of the total mass; the reducing agent is activated carbon, and its amount is 5% of the total slag; the amount of added quartz powder is controlled to be 6:1 in the ratio of silicon to aluminum. After the materials are fully mixed, add water with a total amount of 25% of the total mass of the raw materials to the mixture, and mix it evenly through stirring or agitator and other equipment to ensure that the materials form a mixture with good viscosity and plasticity. The mixed material is balled using a disc ball making machine, and the particle size of the raw ball is controlled to be about 15mm to form a uniform ceramsite raw ball. After the molding is completed, the spheres are placed in an oven for full drying. The oven is set at a temperature of 105°C and the drying time is not less than 1.5 hours until the moisture content of the raw ball is less than 3%. During the pyrometallurgical process, a small rotary atmosphere furnace is charged with argon gas, and the temperature is raised from room temperature to the set temperature at 10°C / min, and the roasting temperature is set to 900°C. The roasting time is controlled to 30min, 45min and 60min respectively to ensure that the material reacts fully. After the roasting is completed, the furnace is cooled and the ceramsite is taken out after the temperature drops below 500°C, completing the preparation of ceramsite and realizing the recycling of resources and environmental protection. The specific data are shown in Table 6 below.

[0041] Table 6 Effect of calcination time on the properties of ceramsite

[0042]

[0043] Example 5

[0044] The arsenic alkali leaching slag and fly ash are crushed and ground to a particle size of less than -50 mesh. 500g of arsenic alkali leaching slag and 100g of fly ash are weighed after the crushing and grinding. The arsenic alkali leaching slag and fly ash are mixed with SiO2, binder and reducing agent in a certain proportion. The binder is bentonite, and its mass percentage content is 10% of the total mass; the reducing agent is activated carbon, and its amount is 5% of the total slag; the amount of added quartz powder is controlled to be 6:1 in the ratio of silicon to aluminum. After the materials are fully mixed, add water with a total amount of 25% of the total mass of the raw materials to the mixture, and mix it evenly through stirring or agitator and other equipment to ensure that the materials form a mixture with good viscosity and plasticity. Use a disc ball making machine to ball the mixture, and control the raw ball particle size to be about 5mm, 15mm and 25mm respectively to form a uniform ceramsite raw ball. After forming, the spheres are placed in an oven for thorough drying. The oven temperature is set at 105°C and the drying time is not less than 1.5 hours, until the moisture content of the raw balls is less than 3%. During the pyrometallurgical process, a small rotary atmosphere furnace is charged with argon gas, and the temperature is raised from room temperature to the set temperature at a rate of 10°C / min. The roasting temperature is set to 900°C. The roasting time is set to 45 minutes to ensure that the material reacts fully. After roasting, the furnace is cooled and the ceramsite temperature is taken out after it drops below 500°C, completing the preparation of the ceramsite and realizing resource recycling and environmental protection. The specific data are shown in Table 7 below.

[0045] Table 7 Effect of raw ball size on ceramsite performance

[0046]

Claims

1. A method for preparing ceramsite by arsenic alkali leaching residue and fly ash. Features: Arsenic alkali leaching residue and fly ash are subjected to dry ball milling, and then pelletized with silicon dioxide, a binder, a carbonaceous reducing agent and water through a disc pelletizing machine to obtain ceramsite raw material; the ceramsite raw material is dried and roasted to obtain ceramsite.

2. The method for preparing ceramsite by arsenic alkali leaching residue and fly ash according to claim 1, Features: The mass ratio of the arsenic alkali leaching residue to the fly ash is 4 to 6:

1.

3. The method for preparing ceramsite by arsenic alkali leaching residue and fly ash according to claim 1 or 2, Features: The arsenic alkali leaching residue and the fly ash are ball-milled to a particle size of less than 50 meshes.

4. The method for preparing ceramsite by arsenic alkali leaching residue and fly ash according to claim 1, Features: The amount of silicon dioxide used is to adjust the silicon-aluminum mass ratio in the system to 5:1 to 8:1; The amount of the carbonaceous reducing agent is 5% to 8% of the total mass of the arsenic alkali leaching residue and the fly ash; The amount of the binder used is 3-7% of the total mass of the ceramsite raw material.

5. The method for preparing ceramsite by arsenic alkali leaching residue and fly ash according to claim 4, Features: The carbonaceous reducing agent includes at least one of activated carbon and coal; The binder includes at least one of bentonite, aluminum dihydrogen phosphate and water glass.

6. The method for preparing ceramsite by synergistically using arsenic alkali leaching residue and fly ash according to claim 1, Features: The particle size of the ceramsite raw material is controlled between 5 and 25 mm.

7. A method for preparing ceramsite by synergistically using arsenic alkali leaching residue and fly ash according to claim 1, 2, 4, 5 or 6, Features: The drying conditions are as follows: temperature of 100-110° C. and time of 1.5-2.0 h.

8. A method for preparing ceramsite by synergistically using arsenic alkali leaching residue and fly ash according to claim 1, 2, 4, 5 or 6, Features: The calcination conditions are as follows: calcination temperature is 800-1000° C., heating rate is 5-15° C. / min, and time is 30-60 min.

Citation Information

Patent Citations

  • Lightweight and high-strength ceramsite, preparation method and application thereof

    CN112430066A

  • Preparation method of solid waste-based special-shaped ceramsite

    CN116655353A

  • Method for synergistically smelting arsenic alkali residue leaching residues and tungsten-containing waste residues

    CN118389836A

  • Method for preparing ceramsite by using municipal sludge as raw material

    US20200048147A1

Cited By

  • Pelletizing method and device for inhibiting volatilization of arsenic in sintered ceramsite

    CN120423890A