Preparation method and application of bismuth-based lead-free perovskite quantum dot material capable of stably and efficiently emitting light
By using FAX and BiX3 as precursors in the preparation of lead-free perovskite quantum dots and adding oleic acid and oleamine as stabilizers, the fluorescence intensity and color of the quantum dots were successfully regulated, and the regulation in the prior art was solved The problem of difficulty and insufficient fluorescence intensity has achieved stable and efficient preparation of bismuth-based perovskite quantum dot materials, which are suitable for a variety of optoelectronic devices.
Patent Information
- Application Number
- CN202310529740.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the process of preparing lead-free perovskite quantum dots is difficult to accurately regulate the luminous color and fluorescence intensity, which limits its application in optoelectronic devices.
Using FAX and BiX3 as precursors, by dissolving FAX in a mixed solution of DMF and DMSO, and dissolving BiX3 in ethyl acetate, adding oleic acid and oleamine as stabilizers, the nucleation and growth of quantum dots are controlled and their Fluorescence intensity and color, FA3Bi2X9 bismuth-based perovskite quantum dots were produced.
A bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence is achieved, with high fluorescence intensity and stability, suitable for detectors, solar cells and LED devices.
Smart Images

Figure CN118930457A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of quantum dot materials, and in particular to a preparation method and application of a bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence. Background Art
[0002] Lead-free perovskite quantum dots are a new type of semiconductor material that has broad application prospects in solar cells and other optoelectronic devices due to its green environmental protection and high stability.
[0003] In the prior art, the application number is CN202010444236.X, the publication date is October 28, 2022, and the name is "A lead-free perovskite quantum dot and its in-situ conversion synthesis method and application". By adding alcohols to Cs3Cu2I5 nanocrystals, the quantum dot 0D-Cs3Cu2I5 is converted into the quantum dot 1D-CsCu2I3, and the amount of alcohol added in the above process is regulated to accurately adjust the ratio of 0D-Cs3Cu2I5 and 1D-CsCu2I3 mixed nanocrystals, thereby achieving precise adjustment of the luminescent color and realizing adjustable luminescent color between blue-white-yellow. Although the above process can obtain quantum dots that emit light of the desired color, the regulation process of obtaining quantum dots of a specific color requires precise regulation, which makes the preparation difficult and the process complicated. In addition, the essence of the above process is to use alcohols to achieve in-situ conversion of Cs3Cu2I5 nanocrystals to achieve the regulation of the color of quantum dots, but since the process does not regulate the fluorescence intensity and fluorescence quantum yield of the obtained quantum dots, it also limits the application of quantum dots.
[0004] In addition, in the prior art, the application number is CN202010573783.8, the publication date is September 15, 2020, and the name is "An aqueous perovskite quantum dot ink for inkjet printing", which discloses the use of formamidine halide and bismuth halide as precursors, together with water-soluble polymers to prepare aqueous perovskite quantum dot inks, and the polymers are used to coat quantum dots to form a composite with quantum dots, thereby improving the film-forming properties of quantum dot inks. The above process mainly focuses on the water solubility and dispersibility of quantum dots, but does not consider the application of quantum dots in optoelectronic devices.
[0005] In view of this, it is necessary to design an improved preparation method and application of bismuth-based lead-free perovskite quantum dot materials with stable and efficient luminescence to solve the above problems. Summary of the invention
[0006] The purpose of the present invention is to provide a preparation method and application of a bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence.
[0007] To achieve the above-mentioned object of the invention, the present invention provides a method for preparing a bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence, comprising the following steps:
[0008] S1, dissolving FAX in a mixed solution of DMF and DMSO to obtain a first precursor solution; dissolving BiX3 in an ethyl acetate solution to obtain a second precursor solution; wherein FAX is FACl, FABr or FAI; and BiX3 is BiCl3, BiBr3 or BiI3;
[0009] S2. After mixing the first precursor solution and the second precursor solution obtained in step S1, a first stabilizer is added to obtain a mixed solution; then, under stirring, the mixed solution is quickly injected into a mixture of toluene and the second stabilizer, and after the reaction is completed, a FA3Bi2X9 bismuth-based perovskite quantum dot solution is obtained by centrifugation. After rotary evaporation of the FA3Bi2X9 bismuth-based perovskite quantum dot solution, a FA3Bi2X9 powder is obtained, and the average size of the FA3Bi2X9 bismuth-based perovskite quantum dots is 4-6nm.
[0010] Preferably, in step S2, the first stabilizer is one of oleic acid and octanoic acid, and the second stabilizer is one of oleylamine and octylamine.
[0011] Preferably, the ratio of the added amount of the oleic acid to the added amount of the oleylamine is 25:(0.5-1).
[0012] Preferably, in step S1, the concentration of FAX in the first precursor solution is 0.2-0.4 mmol, and the concentration of BiX3 in the second precursor solution is 0.2-0.4 mmol.
[0013] Preferably, in step S2, the molar mass ratio of FAX to BiX3 in the mixed solution is (5-2):2.
[0014] Preferably, in step S2, the stirring temperature is 30-50°C and the stirring time is 20-30 min.
[0015] Preferably, in step S2, the centrifugal speed is 6000-10000 r / min, and the time is 3-6 min.
[0016] Preferably, in step S2, the temperature of the rotary evaporation treatment is 80-90°C and the time is 10-14h.
[0017] Preferably, the bismuth-based lead-free perovskite quantum dot material can be applied to detectors, solar cells, LED devices and other fields.
[0018] Beneficial effects of the present invention:
[0019] 1. The preparation method of the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material provided by the present invention is to mix the precursor solution, mix it with the first stabilizer oleylamine, and then mix it with a mixture of toluene and oleic acid, so as to use toluene to provide a reaction site for the process of generating quantum dots, and use oleylamine and oleic acid as stabilizers and surfactants to jointly control the nucleation and growth of quantum dots, and effectively passivate the surface defects of quantum dots; in addition, in the above process, the fluorescence intensity and color of the quantum dots can be controlled by regulating the ratio of the two precursors, the type of halogen elements in the precursors, and the amount of stabilizer added. Through the above process, FA3Bi2X9 bismuth-based perovskite quantum dots with high fluorescence intensity, stable performance, and high fluorescence quantum yield are obtained.
[0020] 2. The preparation method of the bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence provided by the present invention, by adding oleylamine and oleic acid in steps, utilizing the difference in adsorption between the two and the quantum dots, regulating the nucleation and growth process of the quantum dots, and adjusting the addition amount of each raw material in the preparation process, to obtain quantum dots with an average size of 4-6nm, ensuring that the obtained quantum dots can still maintain the stability and high fluorescence intensity of the quantum dots themselves when applied to luminescent materials, and can emit colors and luminescence ranges that meet application requirements. The FA3Bi2X9 bismuth-based perovskite quantum dots prepared by the above method can be applied to detectors, solar cells, LED devices and other fields, providing an effective method for the application of lead-free perovskite quantum dot materials in the field of luminescence. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the XRD pattern of FA3Bi2Br9 perovskite quantum dots prepared in Example 1 of the present invention;
[0022] Figure 2 TEM image of FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in Example 1 of the present invention;
[0023] Figure 3 This is an XPS graph of FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in Example 1 of the present invention;
[0024] Figure 4 The fluorescence spectrum and absorption spectrum of FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in Example 1 of the present invention;
[0025] Figure 5 The FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in Example 1 of the present invention are used for the relevant characterization of LED devices;
[0026] Figure 6The fluorescence spectra of FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in Examples 1 to 3 of the present invention;
[0027] Figure 7 The fluorescence spectra of FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in Examples 1 and 4 to 5;
[0028] Figure 8 The fluorescence spectra and absorption spectra of the FA3Bi2X9 quantum dot solutions of different halogen species prepared in Example 1;
[0029] Fig. 9 Fluorescence spectra of FA3Bi2Br9 bismuth-based perovskite quantum dots prepared for Example 1, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0032] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0033] See also Figure 1 As shown, the present invention provides a method for preparing a bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence, which specifically comprises the following steps:
[0034] S1, dissolving FAX (formamidine halide) in a mixed solution of DMF and DMSO to obtain a first precursor solution; dissolving BiX3 (bismuth halide) in an ethyl acetate solution to obtain a second precursor solution;
[0035] S2. After mixing the first precursor solution and the second precursor solution prepared in step S1, a first stabilizer is added to obtain a mixed solution; then, under stirring, the mixed solution is quickly injected into a mixture of toluene and the second stabilizer. After the reaction is completed, a FA3Bi2X9 bismuth-based perovskite quantum dot solution is obtained by centrifugation. After rotary evaporation of the FA3Bi2X9 bismuth-based perovskite quantum dot solution, FA3Bi2X9 powder is obtained. The average size of the FA3Bi2X9 bismuth-based perovskite quantum dots is 4-6nm.
[0036] Preferably, in step S1, FAX is FACl, FABr or FAI; BiX3 is BiCl3, BiBr3 or BiI3.
[0037] Preferably, in step S1, the concentration of the first precursor solution is 0.2-0.4 mmol; the concentration of the second precursor solution is 0.2-0.4 mmol.
[0038] Preferably, in step S2, the molar mass ratio of FAX to BiX3 in the mixed solution is (5-2):2.
[0039] Preferably, in step S2, the first stabilizer is one of oleic acid and octanoic acid, and the second stabilizer is one of oleylamine and octylamine. The first stabilizer and the second stabilizer can also play the role of surfactants; preferably, the ratio of the amount of oleic acid in the mixture of toluene and oleic acid to the amount of oleylamine added is 25:(0.5-1).
[0040] Preferably, in step S2, the stirring temperature is 30-50°C and the stirring time is 20-30 min.
[0041] Preferably, in step S2, the rotation speed of the centrifugal process is 6000-10000 r / min, and the time is 3-6 min; the temperature of the rotary evaporation treatment is 80-90° C., and the time is 10-14 h.
[0042] In particular, the FA3Bi2X9 bismuth-based perovskite quantum dots prepared by the above method can be used in detectors, solar cells, LED devices and other fields.
[0043] The following is a further description of the preparation method of the bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence proposed by the present invention in conjunction with specific embodiments:
[0044] Example 1
[0045] In this embodiment, FA3Bi2Br9 bismuth-based perovskite quantum dots were prepared, and the specific preparation method is as follows:
[0046] S1, dissolving 0.4 mmol of FABr in a mixed solution of 1.8 mL of DMF and 0.2 mL of DMSO to prepare a first precursor solution; dissolving 0.268 mmol of BiBr3 in 2 mL of ethyl acetate solution to prepare a second precursor solution;
[0047] The preparation of FABr is carried out according to the following steps: 2 mol of formamidine acetate is dissolved in 2 mol of HBr, placed in a 250 mL round-bottom flask, and stirred at 0°C for 30 min until the formamidine acetate is completely dissolved; then, the solution is evaporated at 100°C using a rotary evaporator, the product is washed with ether, and dried in a vacuum drying oven at 60°C for 24 h to obtain FABr;
[0048] S2, after mixing the first precursor solution and the second precursor solution prepared in step S1, 25 μL of oleylamine was added to obtain a mixed solution; then, under stirring, the mixed solution was quickly injected into a mixture of toluene and oleic acid, the volume of toluene in the mixture was 2 mL, the ratio of oleic acid to oleylamine added was 25:1, oleic acid and oleylamine were used as stabilizers and surfactants, after the reaction was completed, centrifuged at 8000 r / min for 5 min to obtain a FA3Bi2X9 bismuth-based perovskite quantum dot solution, and the FA3Bi2X9 bismuth-based perovskite quantum dot solution was rotary evaporated to obtain FA3Bi2X9 powder, and the average size of the FA3Bi2X9 bismuth-based perovskite quantum dots was 4-6 nm. Wherein, the stirring temperature was 40 ° C and the time was 30 min.
[0049] The XRD pattern of FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in this example is shown in FIG. Figure 1 As shown in the figure, it can be seen that the XRD peak position of the FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in this embodiment is consistent with the peak position of the FA3Bi2Br9 standard XRD card, and the results show that the FA3Bi2Br9 bismuth-based perovskite quantum dots have been successfully prepared; the TEM image and HRTEM image of the FA3Bi2Br9 bismuth-based perovskite quantum dots are shown in Figure 2 As shown in the figure, it can be seen that the FA3Bi2Br9 bismuth-based perovskite quantum dots are in a quasi-spherical shape, and the quantum dots are evenly dispersed without agglomeration; the XPS graph of the FA3Bi2Br9 bismuth-based perovskite quantum dots is shown in Table 3, from which the characteristic peaks of Bi and Br can be clearly seen. The analysis shows that the atomic ratio of Br / Bi in the sample is 4.9, which is higher than their own atomic stoichiometric ratio (Br / Bi=4.5), which indicates that the surface of the quantum dots contains rich Br elements. This result further proves that both Bi and Br elements are stably present in the quantum dots in their respective chemical states.
[0050] In order to explore the fluorescence properties of the FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in this example, the fluorescence spectrum and absorption spectrum of the FA3Bi2Br9 quantum dot solution were tested during the experiment. The excitation light during the test was 350nm. The fluorescence spectrum and absorption spectrum are shown in Figure 2. Figure 4As shown, it can be seen from the figure that the emission wavelength of FA3Bi2Br9 quantum dots is about 437nm, the emission half-width is 65nm, and its absorption peak is located at 404nm, from which the Stokes shift of the sample can be calculated to be 231meV. The results show that the self-absorption effect of the FA3Bi2Br9 bismuth-based perovskite quantum dots prepared in this embodiment is very weak, and it is very suitable as a fluorescent material. In addition, the FA3Bi2Br9 bismuth-based perovskite quantum dot solution emits bright blue light under ultraviolet light excitation, and the fluorescence quantum yield of the quantum dots obtained by testing is 52%.
[0051] Furthermore, this embodiment also provides an application method of the above-mentioned FA3Bi2Br9 bismuth-based perovskite quantum dots for LED devices, which is specifically carried out as follows: take an appropriate amount of FA3Bi2Br9 quantum dot solution and a polystyrene / toluene solution with a concentration of 0.15g / mL, mix and stir for 120 minutes, and after mixing evenly, apply the mixed solution on the inner wall of the LED cap buckle, dry it in a vacuum drying oven at 80°C for 60 minutes, and after standing for a period of time, cover it on the ultraviolet light chip of the LED device. The structure of the LED device covered with quantum dots is as follows Figure 5 As shown in a, the electroluminescence spectrum of the device is compared with the PL emission spectrum of the quantum dots. Figure 5 As shown in b, it can be seen from the figure that the electroluminescence spectrum of the device is basically consistent with the PL emission spectrum of the quantum dots. The results show that the quantum dots prepared in this embodiment can still maintain their original high fluorescence intensity when applied to LED devices; the working state of the LED device is as follows Figure 5 As shown in Figure c, it can be seen from the figure that the working LED device emits blue light in the range of 430-460nm, which is the same color as the quantum dot solution under ultraviolet light; in addition, the position of the LED device in the CIE 1931 color coordinates is as follows Figure 5 As shown in FIG. d, the results show that the device color code is in the blue light region, which further verifies the applicability of the quantum dots prepared in this embodiment to LED devices.
[0052] Examples 2 to 3
[0053] The only difference between Examples 2 to 3 and Example 1 is that the ratios of FABr and BiBr3 in the mixed solution are 4.5:2 and 2:2 respectively. The other steps are basically the same as those in Example 1 and will not be repeated here. The fluorescence spectra of FA3Bi2Br9 quantum dots prepared at different ratios in Examples 1 to 3 are shown in FIG. Figure 6 As shown in the figure, it can be seen that the fluorescence intensity of quantum dots is related to the ratio of FABr and BiBr3. Under a certain ratio, FA3Bi2Br9 quantum dots with high fluorescence intensity can be produced.
[0054] Examples 4 to 5
[0055] The only difference between Examples 4 to 5 and Example 1 is that in step S2, the ratio of oleic acid to oleylamine is 20:1 and 32:1 respectively. The other steps are basically the same as those in Example 1 and will not be described in detail here. The fluorescence spectra of FA3Bi2Br9 quantum dots prepared under different oleic acid addition amounts in Examples 1 and Examples 4 to 5 are shown in FIG. Figure 7 As shown in the figure, it can be seen that when the amount of oleic acid added is 0.625mL, the FA3Bi2Br9 quantum dots show the highest fluorescence intensity. The results show that adding an appropriate amount of oleic acid can make the perovskite quantum dots show the best optical properties. This is because when the amount of oleic acid added is different, the density of the entire reaction system solution will change. If the density is too small, the surface defects of the quantum dot crystal will not be fully passivated, resulting in poor crystallinity of the crystal, which is manifested as low fluorescence quantum efficiency of the quantum dots; when the solution density is too large, the quantum dot crystals will be coated with oleic acid, which will have an adverse effect on the optical properties of the quantum dots.
[0056] Examples 6 to 7
[0057] The difference between Examples 6 and 7 and Example 1 is that the halogen species in the first precursor solution and the second precursor solution are different from those in Example 1. The other steps are basically the same as those in Example 1 and will not be repeated here. The fluorescence spectra and absorption spectra of quantum dots prepared with different halogen species are shown in FIG. Figure 8 As shown in the figure, it can be seen that FA3Bi2X9 quantum dots can achieve fluorescence emission in the wavelength range of 399 to 526nm, the color of the quantum dot sample is consistent with the position change trend of the emission peak, and the position of the corresponding absorption spectrum is also red-shifted or blue-shifted with the change of the halogen component; the results show that by changing the type and ratio of halogen ions, quantum dots of the expected color can be obtained. The optical properties of the quantum dots prepared in Example 1 and Examples 6 to 7 are shown in Table 1.
[0058] Table 1 Comparison of optical properties of quantum dots prepared in Example 1 and Examples 6 to 7
[0059] project quantum dots PLpeak(nm) FWHM(nm) PLQY(%) Example 1 <![CDATA[FA3Bi2Br9]]> 399 63 39 Example 6 <![CDATA[FA3Bi2Cl9]]> 437 65 52 Example 7 <![CDATA[FA3Bi2I9]]> 526 67 0.2
[0060] Comparative Example 1
[0061] The difference between Comparative Example 1 and Example 1 is that the order of adding oleic acid and oleylamine is different from that in Example 1, and the other steps are basically the same as those in Example 1, which will not be repeated here.
[0062] Comparative Example 2
[0063] After the first precursor solution and the second precursor solution are mixed, they are directly mixed with oleylamine and a mixture of toluene and oleic acid. The other steps are basically the same as those in Example 1 and will not be repeated here. The fluorescence spectra of FA3Bi2Br9 quantum dots prepared in Example 1 and Comparative Examples 1 to 2 are as follows: Fig. 9 As shown, it can be seen from the figure that the quantum dots prepared by Example 1 have a higher fluorescence intensity, because: in Example 1, after the first precursor solution and the second precursor solution are mixed, they are first mixed with oleylamine, and then mixed with a mixture of toluene and oleic acid. In the above process, quantum dots are generated with the mixing reaction of the first precursor solution and the second precursor solution. At this time, oleylamine combines with the quantum dots and attaches to the surface of the quantum dots, changing the surface activity of the quantum dots; and after adding oleic acid, since the adsorption between oleic acid and quantum dots is stronger than the adsorption between quantum dots and oleylamine, oleic acid is adsorbed to the surface of quantum dots, which produces a passivation effect on the surface of quantum dots, effectively improving the stability and fluorescence quantum efficiency of quantum dots; in addition, the above-mentioned step-by-step addition of oleylamine and oleic acid can realize the control of the nucleation and growth process of quantum dots, ensuring that the final FA3Bi2Br9 quantum dots are evenly dispersed and have high fluorescence intensity. The experimental results further show that the quantum dots prepared by the preparation method of the present invention exhibit a higher fluorescence quantum efficiency (52%).
[0064] In summary, the preparation method and application of the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material proposed in the present invention are as follows: after mixing the precursor solution, mixing it with the first stabilizer oleylamine, and then mixing it with a mixture of toluene and oleic acid, to use toluene to provide a reaction site for the process of generating quantum dots, using oleylamine and oleic acid as stabilizers and surfactants to jointly control the nucleation and growth of quantum dots, and effectively passivate the surface defects of quantum dots; in addition, in the above process, the fluorescence intensity and color of the quantum dots can be controlled by regulating the ratio of the two precursors, the type of halogen elements in the precursors, and the amount of stabilizer added. Through the above process, FA3Bi2X9 bismuth-based perovskite quantum dots with high fluorescence intensity, stable performance, and high fluorescence quantum yield are obtained.
[0065] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence, It is characterized in that The steps include: S1, dissolving FAX in a mixed solution of DMF and DMSO to prepare a first precursor solution; dissolving BiX 3 dissolved in ethyl acetate solution to obtain a second precursor solution; wherein FAX is FACl, FABr or FAI; BiX 3 BiCl 3 、BiBr 3 or BiI 3 ; S2, after mixing the first precursor solution and the second precursor solution prepared in step S1, adding a first stabilizer to obtain a mixed solution; then, under stirring, quickly injecting the mixed solution into a mixture of toluene and the second stabilizer, after the reaction is completed, centrifuging to obtain FA 3 Bi 2 X 9 Bismuth-based perovskite quantum dot solution, the FA 3 Bi 2 X 9 After rotary evaporation of the bismuth-based perovskite quantum dot solution, FA was obtained. 3 Bi 2 X 9 Powder, FA 3 Bi 2 X 9 The average size of bismuth-based perovskite quantum dots is 4-6nm.
2. The method for preparing the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material according to claim 1, It is characterized in that In step S2, the first stabilizer is one of oleic acid and octanoic acid, and the second stabilizer is one of oleylamine and octylamine.
3. The method for preparing the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material according to claim 2, It is characterized in that The ratio of the added amount of the oleic acid to the added amount of the oleylamine is 25:(0.5-1).
4. The method for preparing the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material according to claim 1, It is characterized in that In step S1, the concentration of FAX in the first precursor solution is 0.2-0.4 mmol, and the concentration of BiX in the second precursor solution is 0.2-0.4 mmol. 3 The concentration is 0.2-0.4mmol.
5. The method for preparing the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material according to claim 1, It is characterized in that In step S2, FAX and BiX in the mixed solution 3 The molar mass ratio is (5-2):
2.
6. The method for preparing the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material according to claim 1, It is characterized in that In step S2, the stirring temperature is 30-50°C and the stirring time is 20-30 minutes.
7. The method for preparing the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material according to claim 1, It is characterized in that In step S2, the centrifugal speed is 6000-10000 r / min, and the time is 3-6 min.
8. The method for preparing the stable and efficient luminescent bismuth-based lead-free perovskite quantum dot material according to claim 1, It is characterized in that In step S2, the temperature of the rotary evaporation treatment is 80-90°C and the time is 10-14h.
9. Use of the bismuth-based lead-free perovskite quantum dot material with stable and efficient luminescence according to any one of claims 1 to 8, It is characterized in that The bismuth-based lead-free perovskite quantum dot material can be applied to detectors, solar cells, LED devices and other fields.
Citation Information
Patent Citations
Preparation method of Bi-based perovskite quantum dot material
CN106433619A
Synthetic method of organic inorganic hybrid perovskite quantum point
CN109385268A
Method for stabilizing perovskite nanocrystal by using diamino ligand and perovskite nanocrystal stabilized by diamino ligand
CN114058366A