Polycarboxylate superplasticizer and preparation method thereof

By adding hollow porous nano-silicon oxide and other components to the polycarboxylic acid water reducing agent and carrying out specific treatment, the problem of insufficient sustained release performance in the prior art has been solved, significantly improving the duration of the water reducing agent and improving the Its performance in concrete applications.

CN118930756APending Publication Date: 2024-11-12SICHUAN JIAZHAOFENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310525814.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polycarboxylic acid water reducing agents have insufficient sustained release performance, resulting in poor duration of water reducing agents, which limits their promotion in concrete applications.

Method used

The formula includes hollow porous nanosilicon oxide, polyethylene glycol monomethyl ether, unsaturated monomer, initiator, reducing agent and chain transfer agent, and after sonication and heating and stirring, the pH value is controlled to 5~7. , a polycarboxylic acid water reducing agent with excellent sustained release properties was prepared.

Benefits of technology

It significantly improves the sustained release performance of polycarboxylic acid water reducer, extends the duration of the water reducer, and enhances its application value in concrete applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930756A_ABST
    Figure CN118930756A_ABST
Patent Text Reader

Abstract

The invention discloses a polycarboxylate superplasticizer and a preparation method thereof. The polycarboxylate superplasticizer is prepared from the following components in parts by weight: 30 parts of hollow porous nano silicon oxide, 100 parts of polyethylene glycol monomethyl ether, 20 parts of unsaturated monomer, 4 parts of initiator, 1 part of reducing agent, 3-4 parts of chain transfer agent and 100 parts of deionized water. By adding the porous nano silicon oxide, the polycarboxylic acid water reducing agent has excellent slow release performance, the duration time of the water reducing agent is greatly prolonged, and the popularization and application of the product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polycarboxylate water reducers, and in particular to a polycarboxylate water reducer and a preparation method thereof. Background Art

[0002] Polycarboxylate water reducers are widely used in commercial concrete mixing plants and key projects such as bridges, tunnels, highways, ports, and water conservancy projects. In recent years, with the rapid development of my country's economic construction and the huge investment of the country in infrastructure construction, the production and application of polycarboxylate water reducers have provided broad prospects. With the increasing scarcity of high-quality resource materials such as sand and gravel, how to use different low-quality raw materials to mix high-performance concrete is the top priority of concrete admixture research.

[0003] For example, Chinese patent application CN101205127A discloses a formula of a slow-release polycarboxylic acid-based high-performance water reducer and its manufacturing method. The formula includes an esterification reaction formula and a polymerization reaction formula. The esterification reaction formula uses a portion of maleic anhydride, polyethylene glycol monomethyl ether with a molecular weight of 600, a polymerization inhibitor hydroquinone, a catalyst p-toluenesulfonic acid and concentrated sulfuric acid as raw materials. Maleic anhydride, polyethylene glycol monomethyl ether with a molecular weight of 600, a polymerization inhibitor hydroquinone, and a catalyst p-toluenesulfonic acid are first added at 75°C for 2 hours, and then concentrated sulfuric acid is added to continue the constant temperature reaction for 3 hours. The polymerization process is to add the remaining part of maleic anhydride and allyl polyoxyethylene ether (polymerization degree is 26) water into the previous esterification reactor, add water to acrylic acid and sodium methacrylic acid sulfonate to make a solution, and add water to ammonium persulfate to make a solution, and add them dropwise into the reactor respectively, the dropping time is 2 hours, the constant temperature reaction is 1.5 hours, the temperature is lowered to 50°C, liquid alkali is added for neutralization, and a slow-release polycarboxylic acid-based high-performance water reducer is obtained.

[0004] The above invention uses maleic anhydride as a reaction monomer and its hydrolysis speed is very fast, but the sustained release speed is still not very ideal, and the duration of the water reducer is poor, which seriously limits the promotion and application of this type of product. Summary of the invention

[0005] The present invention provides a polycarboxylate water-reducing agent and a preparation method thereof to solve the problems raised in the above background technology.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A polycarboxylate water reducer is prepared by using the following components in parts by weight: 30 parts of hollow porous nano-silicon oxide, 100 parts of polyethylene glycol monomethyl ether, 20 parts of unsaturated monomers, 4 parts of initiators, 1 part of reducing agents, 3-4 parts of chain transfer agents, and 100 parts of deionized water.

[0008] As a further improvement of the technical solution: the unsaturated monomer is at least one of acrylic acid, methacrylic acid, hydroxyethyl acrylate, and hydroxypropyl acrylate.

[0009] As a further improvement of the technical solution: the chain transfer agent is at least one of mercaptopropionic acid, thioglycolic acid, and mercaptoethanol.

[0010] As a further improvement of the technical solution: the initiator is at least one of hydrogen peroxide, ammonium persulfate and potassium persulfate.

[0011] As a further improvement of the technical solution: the reducing agent initiator is at least one of ascorbic acid, ferrous sulfate, and sodium ascorbate.

[0012] The present invention also provides a method for preparing a polycarboxylate water-reducing agent, comprising the following steps:

[0013] S1, first subjecting the hollow porous nano-silica and polyethylene glycol monomethyl ether to ultrasonic treatment, then mixing the hollow porous nano-silica, polyethylene glycol monomethyl ether and deionized water, and heating and stirring for 10 to 20 minutes to obtain a mixed solution A;

[0014] S2, adding unsaturated monomer, chain transfer agent and initiator to the mixed solution A in S1 to obtain a mixed solution B;

[0015] S3, adding sodium hydroxide to the mixed solution B in S2 until the pH of the mixed solution B reaches 5-7, thereby obtaining a polycarboxylic acid-based water reducer.

[0016] As a further improvement of the present technical solution: in S1, the control parameters of the ultrasonic treatment are an ultrasonic frequency of 1.6 to 1.8 MHz and an ultrasonic power of 400 to 500 W.

[0017] As a further improvement of the technical solution: in S1, the heating temperature is 60-70°C, and the stirring speed is 400-600 r / min.

[0018] As a further improvement of the technical solution: in S2, the unsaturated monomer, chain transfer agent and initiator are added dropwise to the mixed solution A in S1 for 2 to 3 hours.

[0019] As a further improvement of the technical solution: in S2, the step of standing for 1 to 2 hours after the dropwise addition is completed.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The invention adds porous nano silicon oxide to make the polycarboxylic acid water reducer have excellent sustained-release performance, greatly improve the duration of the water reducer, and improve the promotion and application of such products.

[0022] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. The specific implementation of the present invention is given in detail by the following embodiments and their accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0024] Figure 1 The present invention provides a schematic structural diagram of a method for preparing a polycarboxylic acid water-reducing agent. DETAILED DESCRIPTION

[0025] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention. The present invention is described in more detail by way of example with reference to the accompanying drawings in the following paragraphs. The advantages and features of the present invention will become clearer according to the following description and claims. It should be noted that the drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0026] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may also be a component centered. When a component is considered to be "connected to" another component, it may be directly connected to the other component or there may also be a component centered. When a component is considered to be "set on" another component, it may be directly set on the other component or there may also be a component centered. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0028] Example 1: A polycarboxylic acid water-reducing agent is prepared using the following components in parts by weight: 30 parts of hollow porous nano-silica, 100 parts of polyethylene glycol monomethyl ether, 20 parts of unsaturated monomers, 4 parts of initiators, 1 part of reducing agents, 3-4 parts of chain transfer agents, and 100 parts of deionized water.

[0029] Specifically, the unsaturated monomer is at least one of acrylic acid, methacrylic acid, hydroxyethyl acrylate, and hydroxypropyl acrylate; the chain transfer agent is at least one of mercaptopropionic acid, thioglycolic acid, and mercaptoethanol; the initiator is at least one of hydrogen peroxide, ammonium persulfate, and potassium persulfate; and the reducing agent initiator is at least one of ascorbic acid, ferrous sulfate, and sodium ascorbate.

[0030] The present invention also provides a method for preparing a polycarboxylate water-reducing agent, comprising the following steps:

[0031] S1, first subjecting the hollow porous nano-silica and polyethylene glycol monomethyl ether to ultrasonic treatment, then mixing the hollow porous nano-silica, polyethylene glycol monomethyl ether and deionized water, heating and stirring for 10 to 20 minutes to obtain a mixed solution A, wherein the control parameters of the ultrasonic treatment are an ultrasonic frequency of 1.6 to 1.8 MHz, an ultrasonic power of 400 to 500 W, a heating temperature of 60 to 70° C., and a stirring speed of 400 to 600 r / min;

[0032] S2, dropwise adding unsaturated monomer, chain transfer agent and initiator to the mixed solution A in S1 to obtain a mixed solution B, the dropping time is 2 to 3 hours, and after the dropping is completed, the mixture is allowed to stand for 1 to 2 hours;

[0033] S3, adding sodium hydroxide to the mixed solution B in S2 until the pH of the mixed solution B reaches 5-7, thereby obtaining a polycarboxylic acid-based water reducer.

[0034] Comparative Example 1

[0035] The invention is prepared by using the following components in parts by weight: 100 parts of polyethylene glycol monomethyl ether, 20 parts of unsaturated monomer, 4 parts of initiator, 1 part of reducing agent, 3-4 parts of chain transfer agent and 100 parts of deionized water;

[0036] The preparation method is as follows: S1, first subjecting polyethylene glycol monomethyl ether to ultrasonic treatment, then mixing the polyethylene glycol monomethyl ether with deionized water, heating and stirring for 10 to 20 minutes to obtain a mixed solution A, wherein the control parameters of the ultrasonic treatment are an ultrasonic frequency of 1.6 to 1.8 MHz, an ultrasonic power of 400 to 500 W, a heating temperature of 60 to 70° C., and a stirring speed of 400 to 600 r / min;

[0037] S2, dropwise adding unsaturated monomer, chain transfer agent and initiator to the mixed solution A in S1 to obtain a mixed solution B, the dropping time is 2 to 3 hours, and after the dropping is completed, the mixture is allowed to stand for 1 to 2 hours;

[0038] S3, adding sodium hydroxide to the mixed solution B in S2 until the pH of the mixed solution B reaches 5-7, thereby obtaining a polycarboxylic acid-based water reducer.

[0039] The slow-release polycarboxylate water-reducing agent prepared in Example 1 and Comparative Example 1 was tested for dispersibility according to GB / T8077-2000 "Test method for homogeneity of concrete admixtures": Southern cement M42.5, water-reducing agent solid content 0.2%, water dosage 87g, the results are shown in Table 1

[0040]

[0041] Table 1

[0042] It can be seen from the data in Table 1 that the net slurry fluidity of the polycarboxylate water-reducing agent prepared in Example 1 of the present invention within 1 hour has excellent sustained-release performance compared with the polycarboxylate water-reducing agent without hollow porous nano-silica, and the duration of the water-reducing agent is greatly improved.

[0043] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A polycarboxylate water reducer, characterized in that: The invention is prepared by using the following components in parts by weight: 30 parts of hollow porous nano-silicon oxide, 100 parts of polyethylene glycol monomethyl ether, 20 parts of unsaturated monomer, 4 parts of initiator, 1 part of reducing agent, 3-4 parts of chain transfer agent and 100 parts of deionized water.

2. A polycarboxylate water reducer according to claim 1, characterized in that: The unsaturated monomer is at least one of acrylic acid, methacrylic acid, hydroxyethyl acrylate, and hydroxypropyl acrylate.

3. A polycarboxylate water reducer according to claim 1, characterized in that: The chain transfer agent is at least one of mercaptopropionic acid, thioglycolic acid and mercaptoethanol.

4. A polycarboxylate water reducer according to claim 1, characterized in that: The initiator is at least one of hydrogen peroxide, ammonium persulfate and potassium persulfate.

5. A polycarboxylate water reducer according to claim 1, characterized in that: The reducing agent initiator is at least one of ascorbic acid, ferrous sulfate and sodium ascorbate.

6. A method for preparing a polycarboxylate water-reducing agent, characterized in that: The following steps are involved: S1, first subjecting the hollow porous nano-silica and polyethylene glycol monomethyl ether to ultrasonic treatment, then mixing the hollow porous nano-silica, polyethylene glycol monomethyl ether and deionized water, and heating and stirring for 10 to 20 minutes to obtain a mixed solution A; S2, adding unsaturated monomer, chain transfer agent and initiator to the mixed solution A in S1 to obtain a mixed solution B; S3, adding sodium hydroxide to the mixed solution B in S2 until the pH of the mixed solution B reaches 5-7, thereby obtaining a polycarboxylic acid-based water reducer.

7. A polycarboxylate water reducer and a preparation method thereof according to claim 6, characterized in that: In S1, the control parameters of the ultrasonic treatment are an ultrasonic frequency of 1.6-1.8 MHz and an ultrasonic power of 400-500 W.

8. A polycarboxylate water reducer and a preparation method thereof according to claim 6, characterized in that: In the above S1, the heating temperature is 60-70°C, and the stirring speed is 400-600 r / min.

9. A polycarboxylate water-reducing agent and a preparation method thereof according to claim 6, characterized in that: In the step S2, the unsaturated monomer, the chain transfer agent and the initiator are added dropwise to the mixed solution A in S1 for 2 to 3 hours.

10. A polycarboxylate water reducer and a preparation method thereof according to claim 6, characterized in that: In S2, after the dropwise addition is completed, the mixture is allowed to stand for 1 to 2 hours.