Fluoride-free waterproof agent and preparation method thereof

By using fluorine-free waterproofing agents formed by monomers such as octadecyl methacrylate, the existing fluorine-free waterproofing agents have solved the problems of stiffness in the hand, poor waterproofing effect, poor washing resistance and larger color, and achieved soft feel and good waterproofing. Effects and wash resistance reduce the sticky roll phenomenon and improve light reflection and refractive effects.

CN118930763APending Publication Date: 2024-11-12GUANGDONG HONGHAO CHEM CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410991375.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing fluorine-free waterproofing agent forms a rigid protective film on the surface of the fabric, affecting the feel, poor waterproofing effect, easy to stick, poor washing resistance, and large color, affecting light reflection and refraction.

Method used

Monomers such as octadecyl methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, monovinyl polydimethylsiloxane and vinyl chloride are formed by emulsification and high-pressure homogenization. The emulsion is added to the initiator for polymerization to form a fluorine-free waterproofing agent with good hydrophobicity, softness and binding strength.

Benefits of technology

It improves the feel, waterproof effect, wash resistance and color of the fluorine-free waterproofing agent, reduces the phenomenon of sticking to the rollers, and improves the light reflection and refractive effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958964220000031
    Figure BDA0004958964220000031
  • Figure BDA0004958964220000071
    Figure BDA0004958964220000071
  • Figure BDA0004958964220000072
    Figure BDA0004958964220000072
Patent Text Reader

Abstract

The invention discloses a fluoride-free waterproof agent and a preparation method thereof, and the preparation method comprises the following steps: (1) adding octadecyl methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, monovinyl polydimethylsiloxane, deionized water, a solvent and an emulsifier into a reaction kettle protected by nitrogen, and heating and stirring; an emulsion with blue light is obtained; (2) carrying out high-pressure homogenization treatment on the emulsion obtained in the step (1); and (3) reacting the emulsion obtained in the step (2) with vinyl chloride, an initiator and a chain transfer agent to obtain the fluoride-free waterproof agent. The fluoride-free waterproof agent prepared by the preparation method disclosed by the invention has the advantages of good hand feeling, waterproof effect, washability and small color change, and the phenomenon of roll sticking is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproofing agents, and in particular relates to a fluorine-free waterproofing agent and a preparation method thereof. Background Art

[0002] The application of water repellents is crucial to improving the performance of textiles, especially in the fields of outdoor clothing, sportswear, rain gear and some household items. Fluorine-containing water repellents have become the leading products in the market in the past few decades due to their excellent hydrophobic and anti-fouling capabilities. However, fluorine-containing water repellents are expensive, the fluorine-containing raw materials used in production consume high energy and cause heavy pollution, and the fluorine-containing substances they carry are difficult to degrade and have bioaccumulation toxicity.

[0003] Faced with the limitations of fluorine-containing waterproofing agents, fluorine-free waterproofing agents, as a more environmentally friendly and healthier choice, are gradually gaining market share. However, in actual applications, there are also some problems after the fabric is finished with a fluorine-free waterproofing agent: a. The polymer in the fluorine-free waterproofing agent forms a protective film on the surface of the fabric, which will affect the natural feel of the fabric and make it more rigid; b. Fluorine-free waterproofing agents are usually composed of non-fluorinated polymers, and their surface tension is relatively high. The higher surface tension means that the waterproofing agent has poor spreading on the surface of the fabric, and may form a discontinuous or uneven thickness film, resulting in poor waterproofing effect of the fluorine-free waterproofing agent; c. During the processing, the fluorine-free waterproofing agent may cause adhesion between the fabric and the equipment roller, which not only affects the production efficiency, but also may damage the fabric and increase the defective rate; d. The chemical bonding strength of the fluorine-free waterproofing agent is lower than that of the fluorine-containing waterproofing agent, and the bonding force between the fluorine-free waterproofing agent and the fabric is relatively weak, so it is more easily destroyed during the washing process. Therefore, the waterproofing effect of the fabric treated with the fluorine-free waterproofing agent will be significantly reduced after multiple washings, and there is a problem of poor washability; e. A thin film formed by the fluorine-free waterproofing agent will seriously affect the reflection and refraction of light on the surface of the fabric, thereby changing the visual effect of the color.

[0004] Therefore, there is an urgent need for a fluorine-free waterproofing agent and a preparation method thereof to solve the deficiencies of the prior art problems. Summary of the invention

[0005] In view of the above problems, the object of the present invention is to provide a fluorine-free waterproofing agent and a preparation method thereof. The fluorine-free waterproofing agent prepared by the preparation method has good hand feel, waterproof effect, washability, small color change, and improved roller sticking phenomenon.

[0006] To achieve the above objectives, the first aspect of the present invention provides a method for preparing a fluorine-free waterproofing agent, comprising the steps of:

[0007] (1) adding octadecyl methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, monovinyl polydimethylsiloxane, water, a solvent, and an emulsifier into a reaction kettle protected by nitrogen, heating and stirring, and obtaining a blue-light emulsion;

[0008] (2) subjecting the emulsion after step (1) to high pressure homogenization;

[0009] (3) reacting the emulsion after step (2) with vinyl chloride, an initiator, and a chain transfer agent to obtain a fluorine-free waterproofing agent.

[0010] Compared with the prior art, the present invention uses octadecyl methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, and monovinyl polydimethylsiloxane as monomers, and with the help of emulsifiers, mechanical stirring and high-pressure homogenization treatment, the monomers are evenly and stably dispersed in water to form an emulsion, and then vinyl chloride and initiators are added for polymerization to generate a fluorine-free waterproofing agent. Among them, octadecyl methacrylate containing a long-chain alkyl group is used to give the fluorine-free waterproofing agent good hydrophobicity and softness, thereby achieving a waterproof effect and soft hand feel; 2-hydroxyethyl methacrylate helps to improve the stability of the emulsion, is beneficial to the subsequent polymerization reaction, and can also reduce the sticking roller phenomenon of the fluorine-free waterproofing agent during the processing; glycidyl methacrylate contains epoxy groups, which can participate in the cross-linking reaction to form a network structure, thereby improving the bonding force between the fluorine-free waterproofing agent and the fabric; the main chain of monovinyl polydimethylsiloxane is composed of alternating silicon and oxygen atoms, and the silicon-oxygen bond is longer than the carbon-carbon bond and has a larger bond angle, which makes the molecular chain have a greater degree of rotational freedom, thereby improving the fluorine-free waterproofing. The flexibility of the water-based agent, while monovinyl polydimethylsiloxane has a long non-polar segment, which also gives the fluorine-free waterproof agent a good low surface energy; polyvinyl chloride itself has a certain mechanical strength, and as a part of the copolymer, it can also enhance the bonding force between the fluorine-free waterproof agent and the fabric, so that the fluorine-free waterproof agent is more firmly attached to the fabric, thereby improving the water resistance; and, with the help of emulsifiers, mechanical stirring and high-pressure homogenization treatment, it is also helpful to improve the stability of the emulsion, which is beneficial to the subsequent polymerization reaction and can also reduce the sticking phenomenon of the fluorine-free waterproof agent during the processing; in addition, the film formed by the fluorine-free waterproof agent of the present invention will not seriously affect the reflection and refraction of light on the surface of the fabric, that is, the color change is small. Therefore, the fluorine-free waterproof agent prepared by the preparation method of the present invention has a good feel, waterproof effect, washability, small color change, and improved sticking phenomenon.

[0011] Specifically, the structural formula of the fluorine-free waterproofing agent of the present invention is as follows:

[0012]

[0013] Among them, x is 16 to 36, y is 4 to 112, z is 4 to 12, m is 4 to 8, and n is 2 to 4.

[0014] Furthermore, the present invention includes, by weight, 10 to 20 parts of octadecyl methacrylate, 1 to 5 parts of 2-hydroxyethyl methacrylate, 1 to 5 parts of glycidyl methacrylate, 1 to 4 parts of monovinyl polydimethylsiloxane, 42.4 to 83.85 parts of water, 1 to 10 parts of solvent, 1.9 to 8 parts of emulsifier, 0.1 to 0.5 parts of vinyl chloride, 0.05 to 0.1 parts of initiator, and 0.1 to 5 parts of chain transfer agent. Specifically, the content of octadecyl methacrylate may be, but not limited to, 10 parts, 12 parts, 15 parts, 18 parts, and 20 parts; the content of 2-hydroxyethyl methacrylate may be, but not limited to, 1 part, 2 parts, 3 parts, 4 parts, and 5 parts; the content of glycidyl methacrylate may be, but not limited to, 1 part, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4..5 parts, and 5 parts; the content of monovinyl polydimethylsiloxane may be, but not limited to, 1 part, 2 parts, 2.5 parts, 3 parts, 3.5 parts, and 4 parts; the content of water may be, but not limited to, 42.4 parts, 43 parts, 48 ​​parts, 54 parts, 60 parts, 63 parts, 66 parts, 70 parts, 74 parts, 78 parts, 80 parts, 82 parts, 83. 85 parts; the content of solvent can be but not limited to 1 part, 3 parts, 6 parts, 9 parts, 10 parts; the content of emulsifier can be but not limited to 1.9 parts, 2.2 parts, 2.8 parts, 3 parts, 3.5 parts, 4.1 parts, 4.6 parts, 5 parts, 5.5 parts, 6.2 parts, 6.8 parts, 7 parts, 7.2 parts, 7.5 parts, 8 parts; the content of vinyl chloride can be but not limited to 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts; the content of initiator can be but not limited to 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts, 0.09 parts, 1.0 parts; the content of chain transfer agent can be but not limited to 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts.

[0015] Furthermore, the emulsifier of the present invention includes at least one of a nonionic emulsifier and a cationic emulsifier.

[0016] Furthermore, the nonionic emulsifier of the present invention includes Tween emulsifier, Span emulsifier, isomeric tridecanol ether; the cationic emulsifier includes octadecyl trimethyl ammonium chloride. Specifically, the Tween emulsifier can be Tween 60, the Span emulsifier can be Span 80, the isomeric tridecanol ether is isomeric tridecanol ether EO7, and the octadecyl trimethyl ammonium chloride is octadecyl trimethyl ammonium chloride 1831.

[0017] Furthermore, the pressure of the high-pressure homogenization treatment of the present invention is 0.1-0.3 MPa; and the time of the high-pressure homogenization treatment is 1-10 min.

[0018] Furthermore, the solvent of the present invention includes at least one of dipropylene glycol, tripropylene glycol, dipropylene glycol ethyl ether and tripropylene glycol ethyl ether.

[0019] Furthermore, the initiator of the present invention is an azo initiator. Specifically, the azo initiator can be azobisisobutylamidine hydrochloride.

[0020] Furthermore, the chain transfer agent of the present invention is an alkyl mercaptan. Specifically, the alkyl mercaptan may be dodecyl mercaptan.

[0021] Furthermore, in step (1) of the present invention, the temperature of heating and stirring is 60-70°C, and the stirring time is 30-50 minutes. Specifically, the temperature of heating and stirring can be but not limited to 60°C, 65°C, 68°C, 70°C; the stirring time can be but not limited to 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes.

[0022] Furthermore, in step (3) of the present invention, the reaction temperature is 65-75°C and the reaction time is 3-4h. The reaction temperature may be, but not limited to, 65°C, 68°C, 71°C, 73°C, 75°C; the reaction time may be, but not limited to, 3h, 3.2h, 3.5h, 3.8h, 4h.

[0023] Correspondingly, the second aspect of the present invention further provides a fluorine-free waterproofing agent, which is prepared by the above-mentioned preparation method of the fluorine-free waterproofing agent.

[0024] Compared with the prior art, the structure of the fluorine-free waterproofing agent of the present invention comprises methacrylate containing a long-chain alkyl group, 2-hydroxyethyl methacrylate, glycidyl methacrylate, monovinyl polydimethylsiloxane and polyvinyl chloride, so the fluorine-free waterproofing agent of the present invention has good hand feel, waterproof effect, washability, small color change and improved roller sticking phenomenon. DETAILED DESCRIPTION

[0025] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0026] Example 1

[0027] This embodiment provides a method for preparing a fluorine-free waterproofing agent, the steps comprising:

[0028] (1) 120 g of octadecyl methacrylate, 12 g of 2-hydroxyethyl methacrylate, 20 g of glycidyl methacrylate, 15 g of monovinyl polydimethylsiloxane, 600 g of deionized water, 20 g of tripropylene glycol, 6 g of octadecyl trimethylammonium chloride 1831, 5 g of Tween 60, 8 g of isomeric tridecyl alcohol ether EO7, and 9 g of Span 80 were added to a reaction kettle protected by nitrogen, heated to 65° C. and stirred for 35 min to obtain a blue-glowing emulsion;

[0029] (2) subjecting the emulsion after step (1) to high pressure homogenization at 0.2 MPa for 8 min;

[0030] (3) The emulsion after step (2) was reacted with 4 g of vinyl chloride, 0.8 g of azobisisobutylamidine hydrochloride, and 5 g of dodecyl mercaptan at 68° C. for 3.5 h to obtain a fluorine-free waterproofing agent.

[0031] Example 2

[0032] This embodiment provides a method for preparing a fluorine-free waterproofing agent, the steps comprising:

[0033] (1) 140 g of octadecyl methacrylate, 18 g of 2-hydroxyethyl methacrylate, 15 g of glycidyl methacrylate, 25 g of monovinyl polydimethylsiloxane, 700 g of deionized water, 40 g of tripropylene glycol, 10 g of octadecyl trimethylammonium chloride 1831, 8 g of Tween 60, 10 g of isomeric tridecyl alcohol ether EO7, and 5 g of Span 80 were added to a reaction kettle protected by nitrogen, heated to 68° C. and stirred for 40 min to obtain a blue-glowing emulsion;

[0034] (2) subjecting the emulsion after step (1) to high pressure homogenization at 0.3 MPa for 6 min;

[0035] (3) The emulsion after step (2) was reacted with 5 g of vinyl chloride, 1 g of azobisisobutylamidine hydrochloride, and 8 g of dodecyl mercaptan at 72° C. for 3.8 h to obtain a fluorine-free waterproofing agent.

[0036] Example 3

[0037] This embodiment provides a method for preparing a fluorine-free waterproofing agent, the steps comprising:

[0038] (1) 180 g of octadecyl methacrylate, 22 g of 2-hydroxyethyl methacrylate, 25 g of glycidyl methacrylate, 30 g of monovinyl polydimethylsiloxane, 780 g of deionized water, 55 g of tripropylene glycol, 12 g of octadecyl trimethylammonium chloride 1831, 12 g of isomeric tridecyl alcohol ether EO7, and 8 g of Span 80 were added to a reaction kettle protected by nitrogen, heated to 70° C. and stirred for 45 min to obtain a blue-glowing emulsion;

[0039] (2) subjecting the emulsion after step (1) to high pressure homogenization at 0.15 MPa for 10 min;

[0040] (3) The emulsion after step (2) was reacted with 4.8 g of vinyl chloride, 1.2 g of azobisisobutylamidine hydrochloride, and 12 g of dodecyl mercaptan at 75° C. for 4 h to obtain a fluorine-free waterproofing agent.

[0041] Comparative Example 1

[0042] This comparative example provides a method for preparing a fluorine-free waterproofing agent, the steps comprising:

[0043] (1) 120 g of octadecyl methacrylate, 12 g of 2-hydroxyethyl methacrylate, 20 g of glycidyl methacrylate, 15 g of vinyl trimethoxysilane, 600 g of deionized water, 20 g of tripropylene glycol, 6 g of octadecyl trimethylammonium chloride 1831, 5 g of Tween 60, 8 g of isomeric tridecyl alcohol ether EO7, and 9 g of Span 80 were added to a reaction kettle protected by nitrogen, heated to 65° C. and stirred for 35 min to obtain a blue-glowing emulsion;

[0044] (2) subjecting the emulsion after step (1) to high pressure homogenization at 0.2 MPa for 8 min;

[0045] (3) The emulsion after step (2) was reacted with 4 g of vinyl chloride, 0.8 g of azobisisobutylamidine hydrochloride, and 5 g of dodecyl mercaptan at 68° C. for 3.5 h to obtain a fluorine-free waterproofing agent.

[0046] Comparative Example 2

[0047] This comparative example provides a method for preparing a fluorine-free waterproofing agent, the steps comprising:

[0048] (1) 120 g of octadecyl methacrylate, 12 g of 3-chloro-2-hydroxy-propyl methacrylate, 20 g of glycidyl methacrylate, 15 g of monovinyl polydimethylsiloxane, 600 g of deionized water, 20 g of tripropylene glycol, 6 g of octadecyl trimethylammonium chloride 1831, 5 g of Tween 60, 8 g of isomeric tridecyl alcohol ether EO7, and 9 g of Span 80 were added to a reaction kettle protected by nitrogen, heated to 65° C. and stirred for 35 min to obtain a blue-glowing emulsion;

[0049] (2) subjecting the emulsion after step (1) to high pressure homogenization at 0.2 MPa for 8 min;

[0050] (3) The emulsion after step (2) was reacted with 4 g of vinyl chloride, 0.8 g of azobisisobutylamidine hydrochloride, and 5 g of dodecyl mercaptan at 68° C. for 3.5 h to obtain a fluorine-free waterproofing agent.

[0051] The fluorine-free waterproofing agent prepared in Examples 1 to 3 and Comparative Examples 1 to 2 was diluted with tap water to a concentration of 30 g / L. Cotton woven fabric, polyester taffeta 290T, and matte nylon 40D were cut into 22*20 cm in length and width, and the mixture was immersed and rolled (170°C × 90s) with a rolling pressure of 3 kg / cm 2 , 5r / min, the water resistance was tested according to the AATCC 22-2017 test standard, and the water resistance was tested according to the AATCC-135 (home washing) standard for 10 washes (HL10). The results are shown in Table 1.

[0052] The unfinished polyester taffeta 290T was placed under the light source D65, and the DL*, Da*, Db*, and DE* of the polyester taffeta 290T were tested by a colorimeter, and the results are shown in Table 2. The polyester taffeta 290T was then finished with the fluorine-free waterproofing agent prepared in Examples 1 to 3 and Comparative Examples 1 to 2. After dipping and rolling, the surface of the roller was observed for adhesion, and then dried in a blast drying oven at 80°C for 10 minutes. The finished polyester taffeta 290T was then placed under the light source D65, and the DL*, Da*, Db*, and DE* were tested by a colorimeter, and the results are shown in Table 2. The hand feel of the unfinished polyester taffeta 290T and the finished polyester taffeta 290T was then tested according to GB / T18318-2001. The shorter the bending length, the softer the hand feel, and vice versa, the harder the hand feel, and the results are shown in Table 2. Then, the peel strength of the finished polyester taffeta 290T was tested according to "FZ / T01010-2012 Determination of peel strength of coated fabrics", and the results are shown in Table 2.

[0053] Table 1

[0054]

[0055] Table 2

[0056]

[0057] It can be seen from Tables 1 and 2 that the fluorine-free waterproofing agent prepared by the preparation method of the present invention has good hand feel, waterproof effect, washability, small color change, and improved roller sticking phenomenon. Comparing Example 1 with Comparative Examples 1 and 2, it can be seen that replacing monovinyl polydimethylsiloxane with vinyl trimethoxysilane or replacing 2-hydroxyethyl methacrylate with 3-chloro-2-hydroxy-propyl methacrylate will affect the stability of the emulsion and affect the hand feel, waterproof effect, washability and color change of the fluorine-free waterproofing agent.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a fluorine-free waterproofing agent, characterized in that the steps include: (1) adding octadecyl methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, monovinyl polydimethylsiloxane, water, a solvent, and an emulsifier into a reaction kettle protected by nitrogen, heating and stirring, and obtaining a blue-light emulsion; (2) subjecting the emulsion after step (1) to high pressure homogenization; (3) reacting the emulsion after step (2) with vinyl chloride, an initiator, and a chain transfer agent to obtain a fluorine-free waterproofing agent.

2. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: Calculated by mass, it includes 10 to 20 parts of octadecyl methacrylate, 1 to 5 parts of 2-hydroxyethyl methacrylate, 1 to 5 parts of glycidyl methacrylate, 1 to 4 parts of monovinyl polydimethylsiloxane, 42.4 to 83.85 parts of water, 1 to 10 parts of solvent, 1.9 to 8 parts of emulsifier, 0.1 to 0.5 parts of vinyl chloride, 0.05 to 0.1 parts of initiator, and 0.1 to 5 parts of chain transfer agent.

3. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: The emulsifier includes at least one of a nonionic emulsifier and a cationic emulsifier.

4. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: The pressure of the high-pressure homogenization treatment is 0.1-0.3 MPa, and the time is 1-10 min.

5. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: The solvent includes at least one of dipropylene glycol, tripropylene glycol, dipropylene glycol ethyl ether and tripropylene glycol ethyl ether.

6. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: The initiator is an azo initiator.

7. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: The chain transfer agent is alkyl mercaptan.

8. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: The heating and stirring in step (1) is performed at a temperature of 60 to 70° C. and for a time of 30 to 50 minutes.

9. The method for preparing a fluorine-free waterproofing agent according to claim 1, characterized in that: The reaction temperature in step (3) is 65-75° C. and the reaction time is 3-4 h.

10. A fluorine-free waterproofing agent, characterized in that: The fluorine-free waterproofing agent is prepared by the preparation method of the fluorine-free waterproofing agent according to any one of claims 1 to 9.

Citation Information

Cited By

  • Cationic polyacrylate waterproof agent dispersion and preparation method thereof

    CN119569933A