Polyurethane sponge hole disordering agent and preparation process thereof

Through modified tetramethylguanidine catalysis and polymerization of oxyalkylene oxidized olefins with different carbon chain lengths, combined with surfactant, a polyurethane sponge pore agent with high pore ratio and controllable pore size was prepared, solving the problems of wear resistance and tear strength , reduces production costs and improves the comprehensive performance of polyurethane sponges.

CN118930805APending Publication Date: 2024-11-12JIANGSU HENGGUANG NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411180622.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyurethane sponge pore agent cannot take into account both wear resistance and tear strength, resulting in an increase in the production cost of polyurethane sponges. The traditional polyether polyol preparation process has oxygen contact problems that affect product quality.

Method used

Modified tetramethylguanidine as catalyst, combined with oxyolefins of different carbon chain lengths to prepare polyether polyols, and with cetyl trimethylammonium bromide and dimethyl silicone oil as surfactants to control the bubble surface Tension and pore size, polyurethane sponge pore agent with high pore rate and controllable pore size was prepared.

Benefits of technology

The porosity and rebound performance of polyurethane sponge are improved, while reducing production costs, ensuring the controllability and comprehensive performance of pore size.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a polyurethane sponge hole chambering agent and a preparation process thereof. The polyurethane sponge hole chambering agent comprises the following components in parts by mass: 40-60 parts of polyether polyol, 20-30 parts of a surfactant and 5-10 parts of deionized water. The polyether polyol is formed by polymerizing an active hydroxyl-containing organic matter and oxyalkylene with different carbon chain lengths. The rebound performance of the product can be improved, the pore diameter of the product can be regulated and controlled, and the application prospect is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical additives, in particular to a polyurethane sponge pore-disordering agent and a preparation process thereof. Background Art

[0002] The pore-disrupting agent is a special type of surfactant, which generally contains hydrophobic and hydrophilic segments or groups. Its function is to reduce the surface tension of the foam, promote the rupture of the cell wall, increase the open porosity of the polyurethane foam, and improve the shrinkage of soft, semi-rigid, and rigid foam products caused by closed cells. The general polyurethane rigid foam has a closed cell structure due to its high crosslinking density and strong cell wall membrane strength during foaming. However, the addition of the pore-disrupting agent makes the obtained foam have sufficient open porosity and a regular and uniform cell structure, which can be used for furniture decoration, sound insulation, filtration and other purposes; semi-rigid foam products can be widely used in products such as automobile roofs. With the development of science and technology, people's demand for open-cell polyurethane rigid foam is increasing.

[0003] The main types of pore-disrupting agents include silicone copolymers, polyamine compounds, lipids, hydrophilic wax dispersions, etc. These pore-disrupting agents can be added to polyurethane sponges to increase the open porosity, but the effect is single and cannot take into account both wear resistance and tear strength. In order to ensure the comprehensive performance of low-density sponges, wear-resistant agents and plasticizers are often added, which increases the production cost of polyurethane sponges. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a polyurethane sponge pore disordering agent and a preparation process thereof.

[0005] The technical solution of the present invention is achieved in this way:

[0006] A polyurethane sponge pore disordering agent, the components of which are: 40-60 parts by weight of polyether polyol, 20-30 parts by weight of surfactant, and 5-10 parts by weight of deionized water;

[0007] The polyether polyol is prepared by polymerizing an organic substance containing active hydroxyl groups and oxidized olefins with different carbon chain lengths.

[0008] Furthermore, the preparation method of the polyether polyol is: placing an organic substance containing active hydroxyl groups in a reaction kettle, adding a catalyst after the reaction conditions are met, and then adding oxidized olefins with different carbon chain lengths for polymerization reaction, and obtaining the polyether polyol after the reaction is completed.

[0009] Polyether polyols are important raw materials for synthesizing polyurethane (PU) and non-ionic surfactants, and are widely used in plastics, rubber, fibers, coatings, adhesives, sealants, footwear, leather, automobiles, construction, metal processing and textiles.

[0010] Polyether polyols are a general term for polymers containing ether repeating units on the main chain and at least 2 hydroxyl groups at the end. According to their monomer composition, they can be divided into three categories: the first category is a polymer obtained by ring-opening polymerization of propylene oxide (PO) and / or ethylene oxide (EO) on active hydrogen compounds as initiators, which are collectively called polyether polyols (PPG). The second category is a polymer that uses PPG as a matrix to make vinyl monomers such as acrylonitrile and styrene polymerize into polymer particles through free radical polymerization and disperse in PPG. This type of polymer is called polymer polyether polyol (POP), which is mainly used to produce PU soft foams and certain elastomers with certain load-bearing performance requirements. The third category is a polymer made by ring-opening polymerization of tetrahydrofuran (THF) on active hydrogen compounds, called polytetrahydrofuran (PTHF) or polytetramethylene ether glycol (PTMEG), which is mainly used to prepare spandex fibers and special elastomers. Among them, PPG is the most widely used.

[0011] Further, the reaction conditions are: 70-90° C., -0.01-0.03 MPa, stirring for 0.5-1 h.

[0012] The general process of polyether polyol polymerization is: raw materials are put into the kettle, vacuum dehydrated, propylene oxide is added after passing the test, the feeding speed is controlled, the feeding is completed, and the materials are aged. In the above steps, some links will cause the materials to contact oxygen in the air, and oxygen has a great influence on the polymerization reaction and the odor of polyether. Dissolved oxygen will oxidize the alcohol hydroxyl group to generate aldehydes, which are further oxidized to produce peroxides. Therefore, the entire reaction needs to be isolated from oxygen.

[0013] Furthermore, the polymerization reaction conditions are: 0.1-0.5Mpa, 100-120°C.

[0014] For the polymerization process, generally increasing the temperature is conducive to the reaction, which can shorten the polymerization reaction time and improve production efficiency. However, since the ring-opening reaction of epoxy compounds is an exothermic reaction, the heat in the reaction process needs to be removed in time, otherwise the heat accumulation will cause the temperature to be uncontrollable, which will bring safety hazards to the equipment and operators.

[0015] Furthermore, the organic compound containing active hydroxyl groups is a diol or a triol.

[0016] Furthermore, the oxidized olefins with different carbon chain lengths are a mixture of olefin oxides.

[0017] Polyether polyols with different carbon chain lengths have different pore expansion effects on polyurethane.

[0018] Furthermore, the catalyst is modified tetramethylguanidine.

[0019] In the traditional PPG preparation process, alkali metal hydroxides such as KOH are often used as polymerization catalysts. However, the use of such catalysts will produce unsaturated double bonds at the ends of the polyethers, thereby affecting the functionality, relative molecular mass and distribution of the product.

[0020] Tetramethylguanidine, TMG for short, is a strong organic base catalyst with a wide range of industrial applications. It is mainly used as a cosolvent for the synthesis of new antibiotic cephalosporins. It can also be used as a catalyst for polyurethane foam. It can also be used for level dyeing of nylon, wool and other proteins to improve their durability.

[0021] Furthermore, the preparation method of the modified tetramethylguanidine is: under the protection of an inert gas, phosphorus oxybromide is added to tetramethylguanidine, heated to reflux reaction, and the modified tetramethylguanidine is obtained after purification.

[0022] During the polymerization process, the active centers of modified tetramethylguanidine and phosphazene salt catalysts are in the form of cations, catalyzing the anionic ring-opening polymerization of propylene oxide. However, compared with phosphazene salt compounds, the synthesis is simpler, without the tedious steps of recrystallization and conversion of different anion salts.

[0023] Furthermore, the surfactant includes hexadecyltrimethylammonium bromide and dimethyl silicone oil.

[0024] During the foaming process, hexadecyl trimethyl ammonium bromide is adsorbed on the surface of the bubbles to control the surface tension of the bubbles. As the gel and foaming proceed, the bubbles are broken at the appropriate time, thereby achieving the purpose of opening the cells.

[0025] The present invention also provides a preparation process of a polyurethane sponge pore-disordering agent, comprising the following steps: placing 40-60 parts by weight of polyether polyol, 20-30 parts by weight of surfactant, and 5-10 parts by weight of deionized water in a container and stirring them uniformly at 40-60° C. to obtain the polyurethane sponge pore-disordering agent.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. Hexadecyltrimethylammonium bromide is adsorbed on the surface of the bubbles to control the surface tension of the bubbles. As the gel and foaming proceed, the bubbles are broken at the appropriate time to achieve the purpose of opening the holes. Polyether polyols can expand the pore size on the basis of opening the holes.

[0028] 2. Polyether polyols with different carbon chain lengths have different effects on pore size, and polyurethane sponges with different but controllable pore sizes can be produced within a certain range.

[0029] 3. While increasing the porosity of the polyurethane sponge, the pore diameter can also be adjusted to improve the rebound performance. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Reagent Description:

[0032] Phosphorus oxybromide, tetramethylguanidine, tetrahydrofuran, glycerol, propylene oxide, butylene oxide, hexadecyltrimethylammonium bromide, dimethyl silicone oil, diphenylmethane diisocyanate, diethanolamine, analytical grade, Sinopharm Chemical Reagent Co., Ltd.; LOD-C, Liming Chemical Research and Design Institute Co., Ltd.

[0033] Preparation Example 1

[0034] Preparation of modified tetramethylguanidine: Under nitrogen protection, 39.3 g of phosphorus oxybromide was added dropwise to 500 mL of tetrahydrofuran solution containing 69.1 g of tetramethylguanidine, and the temperature was raised to 200° C. and refluxed for 4 h. After the reaction was completed, the solution was filtered, and deionized water was added to wash the filtrate. The aqueous phase was separated and evaporated to dryness to obtain the modified tetramethylguanidine.

[0035] Preparation Example 2

[0036] Preparation of polyether polyols: Place 0.5 mol of propylene glycol in a reaction kettle, continue stirring and evacuate at 80°C for 1 hour, add 1.5 g of the modified tetramethylguanidine described in Preparation Example 1, replace with nitrogen three times, continue stirring and evacuate for 0.5 hour, raise the temperature to 110°C, then introduce 5 mol of propylene oxide and 5 mol of butylene oxide, maintain the pressure at 0.3 MPa, react for 30 minutes to obtain the polyether polyol and purify by distillation.

[0037] Example 1

[0038] 60 g of the polyether polyol described in Preparation Example 1, 10 g of hexadecyltrimethylammonium bromide, 15 g of dimethyl silicone oil, and 10 g of deionized water were placed in a container, heated to 50° C., and stirred for 30 minutes to obtain the irregular pore agent.

[0039] 100 g of diphenylmethane diisocyanate, 0.8 g of cross-linking agent diethanolamine, 3.8 g of deionized water, 3 g of pore-disrupting agent, and 0.65 g of catalyst LOD-C were put into a reaction container and mixed evenly, introduced into a mold for mold closing, and demolded after 5 minutes.

[0040] The product has a pore size range of 50-60ppi and a rebound rate of 50%.

[0041] Example 2

[0042] The difference between this embodiment and embodiment 1 is that in the preparation of the polyether polyol, 5 mol of butylene oxide and 5 mol of pentane oxide are used.

[0043] The product has a pore size range of 40-50ppi and a rebound rate of 55%.

[0044] Example 3

[0045] The difference between this embodiment and embodiment 1 is that in the preparation of the polyether polyol, 5 mol of pentyl oxide and 5 mol of hexyl oxide are used.

[0046] The product has a pore size range of 30-40ppi and a rebound rate of 59%.

[0047] Example 4

[0048] The difference between this embodiment and embodiment 1 is that in the preparation of the polyether polyol, 5 mol of hexyl oxide and 5 mol of heptane oxide are used.

[0049] The product has a pore size range of 40-50ppi and a springback rate of 56%.

[0050] Example 5

[0051] The difference between this embodiment and embodiment 1 is that in the preparation of the random polyether polyol, the amount of heptoxide used is 5 mol, and the amount of octoxide used is 5 mol.

[0052] The pore size of the product ranges from 50 to 60 ppi, and the rebound rate is 51%.

[0053] Example 6

[0054] The difference between this embodiment and embodiment 1 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 40 g, and the amount of hexadecyltrimethylammonium bromide used is 20 g.

[0055] The product has a pore size range of 40-50ppi and a rebound rate of 55%.

[0056] Example 7

[0057] The difference between this embodiment and embodiment 2 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 40 g, and the amount of hexadecyltrimethylammonium bromide used is 20 g.

[0058] The product has a pore size range of 30-40ppi and a rebound rate of 60%.

[0059] Example 8

[0060] The difference between this embodiment and embodiment 3 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 40 g, and the amount of hexadecyltrimethylammonium bromide used is 20 g.

[0061] The product has a pore size range of 20-30ppi and a rebound rate of 64%.

[0062] Example 9

[0063] The difference between this embodiment and embodiment 4 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 40 g, and the amount of hexadecyltrimethylammonium bromide used is 20 g.

[0064] The product has a pore size range of 30-40ppi and a rebound rate of 58%.

[0065] Example 10

[0066] The difference between this embodiment and embodiment 5 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 40 g, and the amount of hexadecyltrimethylammonium bromide used is 20 g.

[0067] The product has a pore size range of 40-50ppi and a springback rate of 54%.

[0068] Embodiment 11

[0069] The difference between this embodiment and embodiment 1 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 50 g, and the amount of hexadecyltrimethylammonium bromide used is 15 g.

[0070] The product has a pore size range of 50-60ppi and a rebound rate of 53%.

[0071] Example 12

[0072] The difference between this embodiment and embodiment 2 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 50 g, and the amount of hexadecyltrimethylammonium bromide used is 15 g.

[0073] The product has a pore size range of 40-50ppi and a rebound rate of 58%.

[0074] Embodiment 13

[0075] The difference between this embodiment and embodiment 3 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 50 g, and the amount of hexadecyltrimethylammonium bromide used is 15 g.

[0076] The product has a pore size range of 30-40ppi and a rebound rate of 62%.

[0077] Embodiment 14

[0078] The difference between this embodiment and embodiment 4 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 50 g, and the amount of hexadecyltrimethylammonium bromide used is 15 g.

[0079] The product has a pore size range of 40-50ppi and a rebound rate of 58%.

[0080] Embodiment 15

[0081] The difference between this embodiment and embodiment 5 is that in the preparation of the pore-disrupting agent, the amount of polyether polyol used is 50 g, and the amount of hexadecyltrimethylammonium bromide used is 15 g.

[0082] The product has a pore size range of 50-60ppi and a rebound rate of 54%.

[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A polyurethane sponge pore-disrupting agent, characterized in that: The composition comprises the following components: 40-60 parts by weight of polyether polyol, 20-30 parts by weight of surfactant, and 5-10 parts by weight of deionized water; The polyether polyol is prepared by polymerizing an organic substance containing active hydroxyl groups and oxidized olefins with different carbon chain lengths.

2. The polyurethane sponge pore-disrupting agent according to claim 1, characterized in that: The preparation method of the polyether polyol is as follows: placing an organic substance containing active hydroxyl groups in a reaction kettle, adding a catalyst after the reaction conditions are met, and then adding oxidized olefins with different carbon chain lengths for polymerization reaction, and obtaining the polyether polyol after the reaction is completed.

3. The polyurethane sponge pore-disrupting agent according to claim 2, characterized in that: The reaction conditions are: 70-90°C, stirring at -0.01-0.03 MPa for 0.5-1 h.

4. The polyurethane sponge pore-disrupting agent according to claim 2, characterized in that: The polymerization reaction conditions are: 0.1-0.5Mpa, 100-120°C.

5. The polyurethane sponge pore-disrupting agent according to claim 2, characterized in that: The organic compound containing active hydroxyl groups is diol or triol.

6. The polyurethane sponge pore-disrupting agent according to claim 1, characterized in that: The olefin oxides with different carbon chain lengths are a mixture of olefin oxides.

7. The polyurethane sponge pore-disrupting agent according to claim 2, characterized in that: The catalyst is modified tetramethylguanidine.

8. The polyurethane sponge pore-disrupting agent according to claim 7, characterized in that: The preparation method of the modified tetramethylguanidine is as follows: under the protection of inert gas, phosphorus oxybromide is added to tetramethylguanidine, heated under reflux reaction, and the modified tetramethylguanidine is obtained after purification.

9. The polyurethane sponge pore-disrupting agent according to claim 1, characterized in that: The surfactants include cetyltrimethylammonium bromide and dimethicone.

10. A process for preparing the polyurethane sponge pore-disrupting agent according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: placing 40-60 parts by weight of polyether polyol, 20-30 parts by weight of surfactant and 5-10 parts by weight of deionized water in a container and stirring them uniformly at 40-60° C. to obtain the polyurethane sponge pore-disordering agent.

Citation Information

Patent Citations

  • Application of polyether polyol or polyether polyester as cell opening agent for low resilience polyurethane foam

    CN102336900A

  • Preparation method of polyether polyol

    CN104448287A

  • Method for preparing polyether polyol with low degree of unsaturation, high molecular weight and high activity

    CN104497298A

  • Preparation method of opening agent for high resilience polyurethane foam

    CN105315448A

  • Polyether polyol serving as slow rebound open agent and preparation method of polyether polyol

    CN106117538A

Cited By

  • Intelligent pore disordering agent as well as preparation method and application thereof

    CN122234335A