Preparation method of halogen-free phosphorus-containing flame-retardant epoxy resin

By adding propylene oxide to phosphoric acid in batches under low temperature conditions and carrying out multiple reactions, halogen-free phosphorus-containing flame-retardant epoxy resin is prepared, which solves the problem of flammable epoxy resin and flame retardant affecting material performance, and realizes the problem of epoxy resin flammable and flame retardant affecting material performance. Efficient and environmentally friendly flame retardant effect and stability are improved.

CN118930812APending Publication Date: 2024-11-12DALIAN LIANSHENG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411070956.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The epoxy resin has a low oxygen index and is flammable, which leads to fire hazards. The mechanical properties of the material decrease after the flame retardant are added, making it difficult to prepare epoxy resins with simple operation and good flame retardant effects.

Method used

Propylene oxide was added dropwise to phosphoric acid under low temperature conditions, and after insulation reaction, excess propylene oxide was distilled under reduced pressure to obtain an intermediate phosphorus-containing polyol, then reacted with epoxypropane and catalyst, and slowly added hydrogen The sodium oxide aqueous solution was finally distilled under reduced pressure to obtain a halogen-free phosphorus-containing flame-retardant epoxy resin.

Benefits of technology

Effectively reduce toxic substances during combustion, enhance flame retardant performance and high temperature stability, reduce costs, improve product quality and stability, and is suitable for electronics, electrical and building materials and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980857360000041
    Figure BDA0004980857360000041
  • Figure BDA0004980857360000051
    Figure BDA0004980857360000051
Patent Text Reader

Abstract

The invention discloses a preparation method of halogen-free phosphorus-containing flame-retardant epoxy resin, and relates to the technical field of fine chemical engineering processes, and the preparation method comprises the following steps: dividing excessive propylene oxide into 3-6 batches at a low temperature of 13-17 DEG C, and slowly dropwise adding the excessive propylene oxide into phosphoric acid; after dropwise adding, stirring and heating to 60-120 DEG C, and keeping the temperature to react for 2-10 hours; carrying out reduced pressure distillation to recover excessive epoxypropane to obtain an intermediate phosphorus-containing polyol; the preparation method comprises the following steps: mixing phosphorus-containing polyol with excessive epoxy chloropropane, adding a catalyst, heating to 30-60 DEG C, slowly dropwise adding a sodium hydroxide aqueous solution, and after dropwise adding, carrying out heat preservation reaction at 40-90 DEG C for 2-6 hours; and carrying out reduced pressure distillation to remove excessive epichlorohydrin and water to obtain the halogen-free phosphorus-containing flame-retardant epoxy product. According to the invention, toxic substances during combustion can be effectively reduced, and the environmental protection property is enhanced. And the product contains phosphorus, so that the flame retardant property is improved, and the stability and safety in a high-temperature or combustion environment are enhanced. By accurately controlling the reaction conditions, the preparation process is more accurate and controllable, and the product quality and stability are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fine chemical processes, in particular to a method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin. Background Art

[0002] As a thermosetting material, epoxy resin is widely used in daily life. Due to its excellent electrical properties, physical and mechanical properties, chemical corrosion resistance and bonding properties, it is widely used in electronic and electrical materials, engineering composite materials, coatings, adhesives and matrix materials of composite materials. However, epoxy resin itself has a low oxygen index and is a flammable material. Its limiting oxygen index is only about 18%, which poses a huge fire hazard and limits its application areas. Therefore, it needs to be modified with flame retardants for further use.

[0003] Flame retardant is an additive that makes flammable polymer materials flame retardant. It is widely used in various natural and synthetic polymer materials. When flame retardants are added to polymers, the occurrence of fire can be greatly reduced. Therefore, the research and development of flame retardants plays an important role in protecting human life and property. However, the addition of flame retardants will reduce the mechanical properties of the material itself, or even significantly weaken it.

[0004] Therefore, how to prepare an epoxy resin that is easy to operate, has good flame retardant effect and does not affect the performance of the material itself has become an urgent problem to be solved in the current industry. In view of the above problems, the present invention provides a method for preparing a halogen-free phosphorus-containing flame retardant epoxy resin. Summary of the invention

[0005] In order to solve the above problems, that is, to solve the problems raised by the above background technology, the present invention proposes a preparation method of a halogen-free phosphorus-containing flame-retardant epoxy resin, which comprises S1: dividing excess propylene oxide into 3-6 batches under a low temperature condition of 13-17°C, and slowly dripping it into phosphoric acid; S2: after the dripping is completed, stirring and heating to 60-120°C for insulation reaction for 2-10h; S3: recovering excess propylene oxide by vacuum distillation to obtain an intermediate phosphorus-containing polyol; S4: adding the phosphorus-containing polyol to excess epichlorohydrin and mixing, adding a catalyst, heating to 30-60°C, slowly dripping a sodium hydroxide aqueous solution, and after the dripping is completed, heating at 40-90°C for 2-6h; S5: vacuum distilling off excess epichlorohydrin and water to obtain a halogen-free phosphorus-containing flame-retardant epoxy resin.

[0006] The present invention is further configured as follows: S1, the phosphoric acid is polyphosphoric acid, and the polyphosphoric acid is diluted with 2-4 times of MIBK or EA.

[0007] The present invention is further configured as follows: the material ratio of propylene oxide to polyphosphoric acid in S1 is 4.0-5.0:1, and the material ratio of epichlorohydrin to phosphorus-containing polyol in S4 is 6.5-8.5:1.

[0008] The present invention is further configured as follows: the catalyst described in S4 is one of TBAB, TPAB, TBAI, tetraphenylphosphonium bromide, methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, and triphenylphosphine, and the proportion of the catalyst is 0.05-2wt%.

[0009] The present invention is further configured as follows: the low temperature condition in S1 is preferably 15°C.

[0010] The present invention is further configured as follows: S1 is preferably to divide propylene oxide into 4-5 batches; S2 is preferably to stir and heat to 80-100°C and keep the temperature for reaction for 4-7h; S4 is preferably to heat to between 35-50°C, slowly add sodium hydroxide aqueous solution, and after the addition is completed, keep the temperature at 40-80°C for reaction for 2-5h.

[0011] The present invention is further configured as follows: S1 is more preferably to divide propylene oxide into 5 batches; S2 is more preferably to stir and heat to 80-90°C and keep warm for reaction for 5-6 hours; S4 is more preferably to heat to between 35-45°C, slowly add sodium hydroxide aqueous solution, and after the addition is completed, keep warm for reaction at 50-70°C for 2-4 hours.

[0012] The beneficial technical effects of the present invention are as follows: the epoxy resin prepared by the method of the present invention does not contain halogen, can effectively reduce toxic substances during combustion, and enhance environmental protection. Because the product contains phosphorus, the flame retardant performance is improved, and the stability and safety under high temperature or combustion environment are enhanced. By accurately controlling the reaction conditions, such as temperature, time, and material ratio, the preparation process is made more precise and controllable, and the product quality and stability are improved. The batch addition method is adopted to effectively recover excess reactants, reduce costs, and improve efficiency. The products prepared by the present invention can be widely used in the fields of electronics and electrical, building materials, aerospace, etc., to meet the needs of various industries for flame retardant materials. In summary, the preparation method has the advantages of environmental protection, flame retardancy, process optimization, economic benefits and wide applicability, and is of great significance to the development and application of flame retardant materials. DETAILED DESCRIPTION

[0013] The preferred embodiments of the present invention are described below. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0014] Embodiment 1:

[0015] Add polyphosphoric acid (33.7 g, 0.1 mol) and 84.25 g of methyl isobutyl ketone to a 250 ml four-necked flask equipped with a thermometer, a constant pressure titration funnel, and a reflux condenser. Place the flask in a cold water bath at about 15°C and stir and dilute it evenly. Divide (26.72 g, 0.46 mol) of propylene oxide into 5 portions and slowly add it dropwise to the polyphosphoric acid. After the addition is complete, stir and heat to 85°C. Keep the temperature for 5 hours and recover the excess propylene oxide by distillation under reduced pressure. and diluent, add epichlorohydrin (69.40g, 0.75mol) into the flask and mix, then add 0.45wt% catalyst TBAB, raise the temperature to 35-45°C, slowly add sodium hydroxide aqueous solution, after the addition is completed, keep the temperature at 55-65°C for 4h, distill off the excess epichlorohydrin and water under reduced pressure to obtain a halogen-free phosphorus-containing flame-retardant epoxy product with a viscosity of 132mPa.s, an epoxy equivalent of 156.01mgKOH / g, and a phosphorus content of 6.52%.

[0016] Embodiment 2:

[0017] Add polyphosphoric acid (33.7 g, 0.1 mol) and ethyl acetate 101.10 g to a 250 ml four-necked flask equipped with a thermometer, a constant pressure titration funnel, and a reflux condenser. Place the flask in a cold water bath at about 15°C and stir and dilute it evenly. Divide (29.04 g, 0.50 mol) of propylene oxide into 5 portions and slowly add it dropwise to the polyphosphoric acid. After the addition is complete, stir and heat to 95°C. Keep the temperature for 6 hours and recover the excess propylene oxide by distillation under reduced pressure. and diluent, add epichlorohydrin (74.02g, 0.80mol) into the flask and mix, then add 0.3wt% catalyst TPAB, raise the temperature to 35-45°C, slowly add sodium hydroxide aqueous solution, after the addition is completed, keep the temperature at 65-75°C for 4h, distill off the excess epichlorohydrin and water under reduced pressure to obtain a halogen-free phosphorus-containing flame-retardant epoxy product with a viscosity of 145mPa.s, an epoxy equivalent of 149.93mgKOH / g, and a phosphorus content of 6.20%.

[0018] Embodiment three:

[0019] Add polyphosphoric acid (33.7 g, 0.1 mol) and methyl isobutyl ketone 134.80 g to a 250 ml four-necked flask equipped with a thermometer, a constant pressure titration funnel, and a reflux condenser. Place the flask in a cold water bath at about 15 ° C and stir and dilute it evenly. Divide (23.23 g, 0.40 mol) of propylene oxide into 4 portions and slowly add it dropwise to the polyphosphoric acid. After the addition is complete, stir and heat to 100 ° C, keep the reaction for 4 hours, and recover the excess propylene oxide by vacuum distillation. Propane and diluent, add epichlorohydrin (60.14g, 0.65mol) into the flask and mix, then add 0.2wt% catalyst triphenylphosphine, heat to 45-55℃, slowly add sodium hydroxide aqueous solution, after the addition is complete, keep warm at 60-70℃ for 6h, distill off the excess epichlorohydrin and water under reduced pressure to obtain a halogen-free phosphorus-containing flame-retardant epoxy product with a viscosity of 151mPa.s, an epoxy equivalent of 158.18mgKOH / g, and a phosphorus content of 6.06%.

[0020] Embodiment 4:

[0021] Add polyphosphoric acid (33.7 g, 0.1 mol) and ethyl acetate 134.82 g to a 250 ml four-necked flask equipped with a thermometer, a constant pressure titration funnel, and a reflux condenser. Place the flask in a cold water bath at about 15°C and stir and dilute it evenly. Divide (27.88 g, 0.48 mol) of propylene oxide into 5 portions and slowly drop it into the polyphosphoric acid. After the addition is complete, stir and heat to 110°C. Keep the temperature for 8 hours and recover the excess propylene oxide by distillation under reduced pressure. Alkane and diluent, add epichlorohydrin (64.75g, 0.7mol) into the flask and mix, then add 0.5wt% catalyst TBAI, raise the temperature to 45-55℃, slowly add sodium hydroxide aqueous solution, after the addition is completed, keep the temperature at 55-65℃ for 4h, distill off the excess epichlorohydrin and water under reduced pressure to obtain a halogen-free phosphorus-containing flame-retardant epoxy product with a viscosity of 128mPa.s, an epoxy equivalent of 152.19mgKOH / g, and a phosphorus content of 6.18%.

[0022] Table 1 is the comparative data of the epoxide equivalent, phosphorus content, Tg temperature, limiting oxygen index, and residual carbon content of the phosphorus-containing flame-retardant epoxy resin obtained in Examples 1-4 and the phosphorus-containing flame-retardant epoxy resin on sale, NPEL-128. Among them, LSC203+each resin is used for curing, and the curing is carried out at 80°C*4h; the determination of epoxy equivalent is carried out according to GB / T 4612, and the determination is carried out by point titration method; the determination of limiting oxygen index is carried out according to GB / T 2460-93, and the results are shown in Table 1.

[0023] Table 1. Performance comparison of Examples 1-4 with commercially available products and NPEL-128 product

[0024]

[0025]

[0026] It can be seen from Table 1 that the product provided in Example 1 has a limiting oxygen index of 27.5%, reaches the UL-94V-0 level, reaches the flame retardant material level, and the residual carbon content reaches 29.50%, which can effectively achieve further flame retardant effect. The phosphorus-containing flame retardant epoxy resin of the present invention has good performance in flame retardancy and heat resistance, and the preferred embodiment is significantly improved in various indicators compared with NPEL-128, and the flame retardant performance is significantly stronger than that of the comparative example.

[0027] So far, the technical solutions of the present invention have been described, but it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin, characterized in that: At least: S1: at a low temperature of 13-17°C, add excess propylene oxide in 3-6 batches and slowly dropwise add them into phosphoric acid; S2: After the addition is complete, heat to 60-120°C with stirring and keep reacting for 2-10 hours; S3: recovering excess propylene oxide by distillation under reduced pressure to obtain an intermediate phosphorus-containing polyol; S4: Add excess epichlorohydrin to the phosphorus-containing polyol and mix, then add a catalyst, raise the temperature to 30-60°C, slowly drop a sodium hydroxide aqueous solution, and after the dropwise addition is complete, heat at 40-90°C for 2-6 hours; S5: distill off excess epichlorohydrin and water under reduced pressure to obtain a halogen-free phosphorus-containing flame-retardant epoxy resin.

2. The method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin according to claim 1, characterized in that: S1 The phosphoric acid is polyphosphoric acid, and the polyphosphoric acid is diluted with 2-4 times of MIBK or EA.

3. The method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin according to claim 2, characterized in that: The material ratio of propylene oxide to polyphosphoric acid in S1 is 4.0-5.0:1, and the material ratio of epichlorohydrin to phosphorus-containing polyol in S4 is 6.5-8.5:

1.

4. The method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin according to claim 1, characterized in that: The catalyst described in S4 is one of TBAB, TPAB, TBAI, tetraphenylphosphonium bromide, methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, and triphenylphosphine, and the proportion of the catalyst is 0.05-2wt%.

5. The method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin according to claim 4, characterized in that: The low temperature condition in S1 is preferably 15°C.

6. The method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin according to claim 1, characterized in that: The S1 is preferably to divide the propylene oxide into 4-5 batches; the S2 is preferably to stir and heat to 80-100°C and keep the temperature for reaction for 4-7h; the S4 is preferably to heat to 35-50°C, slowly add sodium hydroxide aqueous solution, and after the addition is complete, keep the temperature at 40-80°C for reaction for 2-5h.

7. The method for preparing a halogen-free phosphorus-containing flame-retardant epoxy resin according to claim 6, characterized in that: The S1 is more preferably to divide the propylene oxide into 5 batches; the S2 is more preferably to stir and heat to 80-90°C and keep the temperature for reaction for 5-6 hours; the S4 is more preferably to heat to between 35-45°C, slowly add sodium hydroxide aqueous solution, and after the addition is completed, keep the temperature at 50-70°C for reaction for 2-4 hours.