Long carbon chain polyamide resin and preparation method thereof

By polymerizing polyamide resins of different viscosity in a melting state, the problem that conventional polyamide resins are difficult to meet the melt strength requirements of large-diameter products is solved, and high melt strength long carbon chain polyamide resins suitable for oil and gas transportation and other fields are prepared. .

CN118930848AActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410995732.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Conventional high viscosity long carbon chain polyamides are difficult to meet the high melt strength requirements of large-diameter products (such as pipelines) during processing, especially when there are high barrier requirements in oil and gas transportation, natural gas transportation, and hydrogen storage and transportation. .

Method used

By polymerizing the first polyamide resin and the second polyamide resin in a melting state, a long carbon chain polyamide resin with high melt strength was prepared. Specifically, the viscosity of the first polyamide resin is 2.0~ 2.3dL/g, the content of end amino and end carboxylic groups is 30 to 60 mmol/kg, the viscosity of the second polyamide resin is 1.5 to 1.8dL/g, and the content of end amino and end carboxylic groups is 20 to 50 mmol/kg, and the content of end amino and end carboxylic groups is 20 to 50 mmol/kg, and the polymerization reaction is carried out.

Benefits of technology

It has achieved the preparation of long carbon chain polyamide resins with high melt strength, meeting the molding requirements of large-diameter products, and is suitable for products in the fields of oil and gas transportation, natural gas transportation, and hydrogen storage and transportation. It has a simple preparation process, mild reaction and high efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960124450000041
    Figure BDA0004960124450000041
  • Figure BDA0004960124450000042
    Figure BDA0004960124450000042
  • Figure BDA0004960124450000131
    Figure BDA0004960124450000131
Patent Text Reader

Abstract

The invention relates to long-carbon-chain polyamide resin and a preparation method thereof, and the method comprises the following steps: carrying out polymerization reaction on first polyamide resin and second polyamide resin in a molten state to prepare the long-carbon-chain polyamide resin, wherein the viscosity of the first polyamide resin is 2.0-2.3 dL / g, the content of amino-terminated groups is 30-60 mmol / kg, and the content of carboxyl-terminated groups is 30-60 mmol / kg; and the viscosity of the second polyamide resin is 1.5-1.8 dL / g, the amino-terminated group content is 20-50 mmol / kg, and the carboxyl-terminated group content is 20-50 mmol / kg. According to the preparation method of the long-carbon-chain polyamide resin disclosed by the embodiment of the invention, the long-carbon-chain polyamide resin with high melt strength can be prepared by carrying out polymerization reaction on two polyamide resins with different viscosities, and the preparation process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to polyamide, in particular to a long carbon chain polyamide resin with higher melt strength and a preparation method thereof. Background Art

[0002] Polyamide (commonly known as nylon) is one of the five general-purpose engineering plastics and is widely used in many fields, such as medical devices, electronic appliances, automobiles, machinery, textiles, industry, new energy and other fields.

[0003] Long-chain polyamide refers to nylon with more than 10 methylene groups between adjacent amide bonds in the main chain of the macromolecule, such as typical varieties such as PA11, PA12, PA1012, and PA1010. PA610 and PA612 do not strictly meet the above definition, but because the length of the diacid exceeds 10 carbons, half of the interval in its periodic length meets the definition of long-chain nylon, while the length of the diamine is only 6 carbons, resulting in the material's temperature resistance and mechanical properties being better than long-chain nylon, and slightly lower than general-purpose nylons PA6 and PA66. Therefore, PA610 and PA612 are often classified as long-chain nylons. Because long-chain polyamide has both the high strength of polyamide and the excellent processing and molding capabilities of polyolefins, and has extremely low water absorption, this gives it performance that is superior to polyethylene, including mechanical properties, heat resistance, pressure resistance, gas barrier properties, etc., so it has better barrier properties than polyethylene in fields that require strict medium tolerance, such as oil and gas transportation, natural gas transportation, and hydrogen storage and transportation.

[0004] However, the above fields usually require large-diameter products (such as pipes), so the raw materials are required to have relatively high melt strength (at least 110mN) during processing, while conventional high-viscosity long-chain polyamides are difficult to meet the above requirements. Summary of the invention

[0005] In order to overcome at least one defect of the above-mentioned prior art, in the first aspect, an embodiment of the present invention provides a method for preparing a long carbon chain polyamide resin, comprising polymerizing a first polyamide resin and a second polyamide resin in a molten state to obtain a long carbon chain polyamide resin; wherein the viscosity of the first polyamide resin is 2.0 to 2.3 dL / g, the terminal amino group content is 30 to 60 mmol / kg, and the terminal carboxyl group content is 30 to 60 mmol / kg; the viscosity of the second polyamide resin is 1.5 to 1.8 dL / g, the terminal amino group content is 20 to 50 mmol / kg, and the terminal carboxyl group content is 20 to 50 mmol / kg.

[0006] In a second aspect, an embodiment of the present invention provides a long carbon chain polyamide resin, which is prepared by the above-mentioned preparation method.

[0007] In the third aspect, an embodiment of the present invention provides a composition for preparing a long carbon chain polyamide, comprising a first polyamide resin and a second polyamide resin, wherein the first polyamide resin has a viscosity of 2.0 to 2.3 dL / g, an end amino group content of 30 to 60 mmol / kg, and an end carboxyl group content of 30 to 60 mmol / kg; the second polyamide resin has a viscosity of 1.5 to 1.8 dL / g, an end amino group content of 20 to 50 mmol / kg, and an end carboxyl group content of 20 to 50 mmol / kg.

[0008] A method for preparing a long carbon chain polyamide resin according to an embodiment of the present invention can prepare a long carbon chain polyamide resin with high melt strength by carrying out a polymerization reaction using two polyamide resins with different viscosities, and the preparation process is simple. DETAILED DESCRIPTION

[0009] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various variations in different embodiments without departing from the scope of the present invention, and the descriptions therein are essentially for illustrative purposes rather than for limiting the present invention. Unless otherwise specified, the pressures referred to herein are absolute pressures.

[0010] One embodiment of the present invention provides a method for preparing a long carbon chain polyamide resin, comprising subjecting a first polyamide resin and a second polyamide resin to a polymerization reaction (or melt polymerization) in a molten state to obtain a long carbon chain polyamide resin; wherein the first polyamide resin has a viscosity of 2.0 to 2.3 dL / g, an amino terminal content of 30 to 60 mmol / kg, and a carboxyl terminal content of 30 to 60 mmol / kg; and the second polyamide resin has a viscosity of 1.5 to 1.8 dL / g, an amino terminal content of 20 to 50 mmol / kg, and a carboxyl terminal content of 20 to 50 mmol / kg.

[0011] In one embodiment, the polyamides of the first polyamide resin and the second polyamide resin are both uncapped polyamides, including an amino group (terminal amino group) and a carboxyl group (terminal carboxyl group) at the end.

[0012] In one embodiment, the viscosity of the first polyamide resin may be 2.0 to 2.3 dL / g, and further may be 2.1 to 2.2 dL / g.

[0013] In one embodiment, the terminal amino group content in the first polyamide resin may be 30 to 60 mmol / kg, and further may be 40 to 50 mmol / kg, for example, 35 mmol / kg, 38 mmol / kg, 42 mmol / kg, 45 mmol / kg, 48 mmol / kg, 52 mmol / kg, 55 mmol / kg, and 58 mmol / kg.

[0014] In one embodiment, the terminal carboxyl content in the first polyamide resin may be 30 to 60 mmol / kg, and further may be 40 to 50 mmol / kg, for example, 35 mmol / kg, 38 mmol / kg, 42 mmol / kg, 45 mmol / kg, 48 mmol / kg, 52 mmol / kg, 55 mmol / kg, and 58 mmol / kg.

[0015] In one embodiment, in the first polyamide resin, the molar ratio of the terminal amino group to the terminal carboxyl group is 0.9 to 1.1:1, for example 1:1.

[0016] In one embodiment, the viscosity of the second polyamide resin is 1.5 to 1.8 dL / g, and may further be 1.6 to 1.7 dL / g.

[0017] In one embodiment, the terminal amino group content in the second polyamide resin may be 20 to 50 mmol / kg, and may further be 30 to 40 mmol / kg, for example, 25 mmol / kg, 28 mmol / kg, 32 mmol / kg, 35 mmol / kg, 38 mmol / kg, 42 mmol / kg, 45 mmol / kg, and 48 mmol / kg.

[0018] In one embodiment, the terminal carboxyl content in the second polyamide resin may be 20 to 50 mmol / kg, and may further be 30 to 40 mmol / kg, for example, 25 mmol / kg, 28 mmol / kg, 32 mmol / kg, 35 mmol / kg, 38 mmol / kg, 42 mmol / kg, 45 mmol / kg, and 48 mmol / kg.

[0019] In one embodiment, in the second polyamide resin, the molar ratio of the terminal amino group to the terminal carboxyl group is 0.9 to 1.1:1, for example 1:1.

[0020] In one embodiment, the mass ratio of the first polyamide resin to the second polyamide resin is 1:(0.3-0.5), for example, 1:0.3, 1:0.4, or 1:0.5.

[0021] In one embodiment, the long carbon chain polyamide resin is a homopolymer, comprising the following structural units:

[0022]

[0023] wherein x is an integer selected from 9 to 11, for example 9, 10 or 11; y is an integer selected from 6 to 18, for example 7, 8, 9, 10, 11, 12, 13, 14, 15, 16 or 17; and z is an integer selected from 8 to 16, for example 9, 10, 11, 12, 13, 14 or 15.

[0024] In one embodiment, the long carbon chain polyamide resin is a homopolymer selected from PA612 (polyamide 612), PA610 (polyamide 610), PA1010 (polyamide 1010), PA1012 (polyamide 1012), PA1212 (polyamide 1212), PA11 (polyundecalactam) or PA12 (polylaurolactam).

[0025] In one embodiment, the first polyamide resin and the second polyamide resin are of the same type and both include the following structural units:

[0026]

[0027] wherein x is an integer selected from 9 to 11, for example 9, 10 or 11; y is an integer selected from 6 to 18, for example 7, 8, 9, 10, 11, 12, 13, 14, 15, 16 or 17; and z is an integer selected from 8 to 16, for example 9, 10, 11, 12, 13, 14 or 15.

[0028] In one embodiment, the first polyamide resin and the second polyamide resin are of the same type, and are both prepared by a polycondensation reaction of a diamine and a dibasic acid or by a ring-opening reaction of a lactam. Further, the first polyamide resin and the second polyamide resin are both selected from PA612, PA610, PA1010, PA1012, PA1212, PA11 or PA12.

[0029] In one embodiment, the reaction temperature of the first polyamide resin and the second polyamide resin is 200-260°C, for example, 205°C, 210°C, 220°C, 230°C, 240°C, 250°C, 255°C.

[0030] In one embodiment, the preparation method of long carbon chain polyamide resin includes: placing raw materials in a reaction container, sealing and heating to maintain pressure for reaction, and then venting and reducing pressure (vacuuming) for reaction; after the reaction is completed, cooling and taking out the material to obtain a long carbon chain polyamide resin with high melt strength.

[0031] In one embodiment, the polymerization reaction process includes: maintaining the reaction system at 200-260° C. and 1.6-2.1 MPa (e.g., 1.7 MPa, 1.8 MPa, 1.9 MPa, 2 MPa) for 1-3 h (e.g., 1.5 h, 2 h, 2.5 h); then venting the system within 1-2 h, and after the pressure in the reaction container drops to normal pressure, evacuating the system until the pressure of the system is less than 1000 Pa, maintaining for 2-4 h (e.g., 3 h) to complete the reaction.

[0032] In one embodiment, the raw materials for preparing the long carbon chain polyamide resin include a first polyamide resin, a second polyamide resin, a solvent and an optional auxiliary agent.

[0033] In one embodiment, the solvent includes one or more of ethanol, methanol, and water. Further, the ratio of the mass of the solvent to the sum of the mass of the first polyamide resin and the second polyamide resin can be 1 to 4:1, for example, 1:1, 2:1, 3:1, 4:1.

[0034] In one embodiment, the auxiliary agent includes an antioxidant, and the oxidant can be one or more of antioxidant 1098, antioxidant 1010, antioxidant 168, and antioxidant 1076. Further, based on the total mass of the first polyamide resin and the second polyamide resin for preparing the long carbon chain polyamide resin as a reference (100%), the amount of the antioxidant can be 0.2 to 0.5 wt‰, for example, 0.3 wt‰, 0.4 wt‰.

[0035] One embodiment of the present invention provides a long carbon chain polyamide resin, which is prepared by the above-mentioned preparation method.

[0036] In one embodiment, the long carbon chain polyamide resin may be in the form of powder and / or granules.

[0037] In one embodiment, the viscosity of the long carbon chain polyamide resin may be 2.4 to 2.9 dL / g, such as 2.5 dL / g, 2.6 dL / g, 2.7 dL / g, or 2.8 dL / g.

[0038] In one embodiment, the melt strength of the long carbon chain polyamide resin is 140 to 210 mN, for example, 140 mN, 142 mN, 143 mN, 145 mN, 148 mN, 150 mN, 155 mN, 160 mN, 161 mN, 165 mN, 170 mN, 175 mN, 178 mN, 180 mN, 185 mN, 190 mN, 193 mN, 195 mN, 200 mN, 201 mN, 202 mN, and 205 mN.

[0039] One embodiment of the present invention provides a composition for preparing a long carbon chain polyamide, comprising the first polyamide resin and the second polyamide resin.

[0040] In one embodiment, the mass ratio of the first polyamide resin to the second polyamide resin contained in the composition for preparing the long carbon chain polyamide is 1:(0.3-0.5), for example, 1:0.4.

[0041] In one embodiment, the composition for preparing the long carbon chain polyamide comprises a first polyamide resin, a second polyamide resin, a solvent and an optional auxiliary agent, wherein the type and amount of the solvent and auxiliary agent can refer to the above description.

[0042] A method for preparing a long carbon chain polyamide resin in one embodiment of the present invention comprises the following steps: using two polyamide resins with different viscosities to carry out a polymerization reaction to obtain a long carbon chain polyamide resin with high melt strength. The long carbon chain polyamide resin can meet the molding requirements of large-diameter products (such as pipelines), and is suitable for preparing products (such as pipelines) in the fields of oil and gas transportation, natural gas transportation, hydrogen storage and transportation, etc.

[0043] In the method for preparing the long carbon chain polyamide resin according to one embodiment of the present invention, the raw materials used can all be existing raw materials and no special preparation is required.

[0044] The method for preparing a long carbon chain polyamide resin according to one embodiment of the present invention has a relatively mild reaction process, high efficiency and simple process.

[0045] The preparation method of the long carbon chain polyamide resin in one embodiment of the present invention has a simple auxiliary agent system and low solvent hazard.

[0046] The following is a further description of the preparation method of the long carbon chain polyamide resin according to one embodiment of the present invention in conjunction with examples. The raw materials and test methods involved in each example and comparative example are as follows.

[0047] raw material

[0048] 1. Polyamide resin

[0049] PA610: produced by Shandong Xianglong New Materials Co., Ltd.; PA1010: produced by Shandong Xianglong New Materials Co., Ltd.; PA1012: produced by Shandong Xianglong New Materials Co., Ltd.; PA11: produced by Arkema (Shanghai) Chemical Co., Ltd.; PA12: produced by Wanhua Chemical Group Co., Ltd.

[0050] 2. Antioxidants

[0051] Antioxidant 1098: produced by Shanghai Aladdin Biochemical Technology Co., Ltd., purity> 99%; Antioxidant 1076: produced by Shanghai Aladdin Biochemical Technology Co., Ltd., purity> 99%; Antioxidant 168: produced by Shanghai Aladdin Biochemical Technology Co., Ltd., purity> 99%; Antioxidant 1010: produced by Shanghai Aladdin Biochemical Technology Co., Ltd., purity> 99%.

[0052] 3. Solvent

[0053] Ethanol: produced by Shanghai McLean Biochemical Technology Co., Ltd., AR analytical grade, purity > 99.5%; Methanol: produced by Shanghai McLean Biochemical Technology Co., Ltd., AR analytical grade, purity > 99.5%; Pure water: homemade by MOLE pure water machine.

[0054] Test Method

[0055] 1. Viscosity

[0056] The viscosity of the polyamide resin was measured by an Ubbelohde viscometer. The equipment model was Zhuoxiang IVS300-6. The sample used for the test was in granular form and the solvent was m-cresol.

[0057] The specific steps are as follows: take an appropriate amount of the resin to be tested, put it into a conical flask after drying, add m-cresol, heat the conical flask to 75°C, and test it on a fully automatic Ubbelohde viscometer (23°C) after the sample is completely dissolved.

[0058] 2. Melt strength

[0059] The melt strength of polyamide resin was measured by melt extensional rheometer according to ISO 16790-2021. The equipment model was Rheotens 71.97. The samples used for the test were in granular form.

[0060] Example 1

[0061] 100 g of the first polyamide resin PA1010 with a viscosity of 2.3 dL / g (the terminal amino group and terminal carboxyl group contents are both 30 mmol / kg) and 30 g of the second polyamide resin PA1010 with a viscosity of 1.8 dL / g (the terminal amino group and terminal carboxyl group contents are both 30 mmol / kg) are added to a 5L reactor, and then 0.026 g of antioxidant 1098 and 260 g of pure water are added thereto.

[0062] After the above addition, the reactor was heated steadily to 210°C, and the pressure was maintained at 1.7MPa for 2 hours; then the air was slowly released for 1.5 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA1010 resin with high melt strength was obtained.

[0063] Example 2

[0064] 100 g of the first polyamide resin PA610 with a viscosity of 2.3 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) and 40 g of the second polyamide resin PA610 with a viscosity of 1.8 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) are added to a 5L reactor, and then 0.056 g of antioxidant 1010 and 300 g of pure water are added thereto.

[0065] After the above addition, the reactor was heated steadily to 250°C, and the pressure was maintained at 2.1MPa for 2 hours; then the air was slowly released for 1.5 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA610 resin with high melt strength was obtained.

[0066] Example 3

[0067] 100 g of the first polyamide resin PA1012 with a viscosity of 2.0 dL / g (the terminal amino group and terminal carboxyl group contents are both 50 mmol / kg) and 50 g of the second polyamide resin PA1012 with a viscosity of 1.5 dL / g (the terminal amino group and terminal carboxyl group contents are both 50 mmol / kg) are added to a 5L reactor, and then 0.075 g of antioxidant 1076 and 600 g of pure water are added thereto.

[0068] After the above addition, the reactor was heated steadily to 220°C, and the pressure was maintained at 2.1MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA1012 resin with high melt strength was obtained.

[0069] Example 4

[0070] 100 g of the first polyamide resin PA12 with a viscosity of 2.2 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) and 40 g of the second polyamide resin PA12 with a viscosity of 1.7 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) were added to a 5L reactor, and then antioxidant 1098, antioxidant 168 (mass ratio of 2:1, a total of 0.042 g) and 520 g of pure water were added thereto.

[0071] After the above addition, the reactor was heated steadily to 210°C, and the pressure was maintained at 2MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA12 resin with high melt strength was obtained.

[0072] Example 5

[0073] 100 g of the first polyamide resin PA1012 with a viscosity of 2.2 dL / g (the terminal amino group and terminal carboxyl group contents are both 30 mmol / kg) and 50 g of the second polyamide resin PA1012 with a viscosity of 1.8 dL / g (the terminal amino group and terminal carboxyl group contents are both 30 mmol / kg) are added to a 5L reactor, and then 0.075 g of antioxidant 1076 and 300 g of pure water are added thereto.

[0074] After the above addition, the reactor was heated steadily to 220°C, and the pressure was maintained at 2.1MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA1012 resin with high melt strength was obtained.

[0075] Example 6

[0076] 100 g of the first polyamide resin PA12 with a viscosity of 2.1 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) and 40 g of the second polyamide resin PA12 with a viscosity of 1.7 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) are added to a 5L reactor, and then 0.042 g of antioxidant 1076 and 300 g of pure water are added thereto.

[0077] After the above addition, the reactor was heated steadily to 200°C, and the pressure was maintained at 1.7MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA12 resin with high melt strength was obtained.

[0078] Example 7

[0079] 100 g of a first polyamide resin PA1010 with a viscosity of 2.2 dL / g (the terminal amino group and terminal carboxyl group contents are both 30 mmol / kg) and 30 g of a second polyamide resin PA1010 with a viscosity of 1.7 dL / g (the terminal amino group and terminal carboxyl group contents are both 30 mmol / kg) were added to a 5L reactor, and then 0.026 g of an antioxidant 1098 and 260 g of an ethanol aqueous solution (the mass ratio of ethanol to water is 1:1) were added thereto.

[0080] After the above addition, the reactor was heated steadily to 210°C, and the pressure was maintained at 1.7MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA1010 resin with high melt strength was obtained.

[0081] Example 8

[0082] 100 g of a first polyamide resin PA1012 with a viscosity of 2.0 dL / g (the terminal amino group and terminal carboxyl group contents are both 60 mmol / kg) and 50 g of a second polyamide resin PA1012 with a viscosity of 1.6 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) were added to a 5L reactor, and then 0.075 g of an antioxidant 1076 and 600 g of a methanol aqueous solution (the mass ratio of methanol to water is 1:2) were added thereto.

[0083] After the above addition, the reactor was heated steadily to 220°C, and the pressure was maintained at 2.1MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA1012 resin with high melt strength was obtained.

[0084] Example 9

[0085] 100 g of a first polyamide resin PA11 with a viscosity of 2.2 dL / g (the terminal amino group and the terminal carboxyl group contents are both 50 mmol / kg) and 40 g of a second polyamide resin PA11 with a viscosity of 1.7 dL / g (the terminal amino group and the terminal carboxyl group contents are both 50 mmol / kg) were added to a 5L reactor, and then antioxidant 1010, antioxidant 168 (mass ratio of 1:1, a total of 0.056 g) and 280 g of ethanol were added thereto.

[0086] After the above addition, the reactor was heated steadily to 220°C, and the pressure was maintained at 2MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA11 resin with high melt strength was obtained.

[0087] Example 10

[0088] 100 g of the first polyamide resin PA1012 with a viscosity of 2.1 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) and 50 g of the second polyamide resin PA1012 with a viscosity of 1.5 dL / g (the terminal amino group and terminal carboxyl group contents are both 60 mmol / kg) are added to a 5L reactor, and then antioxidant 1076, antioxidant 168 (mass ratio of 2:1, a total of 0.045 g) and 600 g of pure water are added thereto.

[0089] After the above addition, the reactor was heated steadily to 220°C, and the pressure was maintained at 2.1MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials, and PA1012 resin with high melt strength was obtained.

[0090] Comparative Example 1

[0091] 100 g of the first polyamide resin PA1012 with a viscosity of 2.0 dL / g (the terminal amino group content is 10 mmol / kg, the terminal carboxyl group content is 60 mmol / kg) and 50 g of the second polyamide resin PA1012 with a viscosity of 1.5 dL / g (the terminal amino group and terminal carboxyl group content are both 60 mmol / kg) are added to a 5L reactor, and then 0.075 g of antioxidant 1076 and 600 g of pure water are added thereto.

[0092] After the above addition, the reactor was heated steadily to 200°C, and the pressure was maintained at 1.7MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials to obtain PA1012 resin.

[0093] Comparative Example 2

[0094] 100 g of the first polyamide resin PA12 with a viscosity of 2.1 dL / g (the terminal amino group and terminal carboxyl group contents are both 40 mmol / kg) and 50 g of the second polyamide resin PA12 with a viscosity of 1.7 dL / g (the terminal amino group content is 10 mmol / kg and the terminal carboxyl group content is 40 mmol / kg) are added to a 5L reactor, and then 0.042 g of antioxidant 1076 and 600 g of pure water are added thereto.

[0095] After the above addition, the reactor was heated steadily to 200°C, and the pressure was maintained at 1.7MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 3 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials to obtain PA12 resin.

[0096] Comparative Example 3

[0097] 100 g of polyamide resin PA1012 with a viscosity of 2.0 dL / g (the content of terminal amino group and terminal carboxyl group is 60 mmol / kg) was added into a 5 L reactor, and then 0.05 g of antioxidant 1076 and 600 g of pure water were added thereto.

[0098] After the above addition, the reactor was heated steadily to 200°C, and the pressure was maintained at 1.7MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 6 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials to obtain PA1012 resin.

[0099] Comparative Example 4

[0100] 100 g of the first polyamide resin PA12 (terminal amino group and terminal carboxyl group content are both 40 mmol / kg) with a viscosity of 2.2 dL / g was added into a 5 L reactor, and then 0.03 g of antioxidant 1076 and 600 g of pure water were added thereto.

[0101] After the above addition, the reactor was heated steadily to 200°C, and the pressure was maintained at 1.7MPa for 2 hours; then the air was slowly released for 2 hours until the pressure in the reactor dropped to normal pressure. After the release, the reactor was evacuated with a vacuum pump until the absolute pressure in the reactor was less than 1000Pa, and maintained for 6 hours. After the reaction was completed, the temperature was lowered and the reactor was opened to take out the materials to obtain PA12 resin.

[0102] The polyamide resins prepared in the examples and comparative examples were pelletized and tested for melt strength. The results are shown in Table 1.

[0103] Table 1

[0104]

[0105]

[0106] According to the data in Table 1, Examples 1 to 10 of the present invention can produce long-chain polyamide resins with high melt strength by using two polyamide resins with different viscosities for polymerization reaction, which meet the molding requirements of large-diameter products and solve the problem that the existing long-chain polyamide is difficult to meet the molding requirements of large-diameter pipes.

[0107] The difference between Comparative Example 3 and Example 3 is that Comparative Example 3 uses only the first polyamide resin for polymerization to prepare high-viscosity polyamide, and the results in Table 1 show that the melt strength of the polyamide resin prepared in Example 3 is much higher than the melt strength of Comparative Example 3. Similarly, the difference between Comparative Example 4 and Example 6 is that Comparative Example 4 uses only the first polyamide resin for polymerization to prepare high-viscosity polyamide, and the results in Table 1 show that the melt strength of the polyamide resin prepared in Example 6 is much higher than the melt strength of Comparative Example 4. This shows that the polymerization reaction of two polyamide resins with different viscosities in the embodiments of the present invention can produce a long carbon chain polyamide resin with high melt strength.

[0108] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.

[0109] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but is only limited by the claims.

Claims

1. A method for preparing a long carbon chain polyamide resin, comprising polymerizing a first polyamide resin and a second polyamide resin in a molten state to obtain a long carbon chain polyamide resin; wherein: The viscosity of the first polyamide resin is 2.0-2.3dL / g, the terminal amino group content is 30-60mmol / kg, and the terminal carboxyl group content is 30-60mmol / kg; the viscosity of the second polyamide resin is 1.5-1.8dL / g, the terminal amino group content is 20-50mmol / kg, and the terminal carboxyl group content is 20-50mmol / kg.

2. The preparation method according to claim 1, wherein The viscosity of the first polyamide resin is 2.1 to 2.2 dL / g; and / or, The viscosity of the second polyamide resin is 1.6-1.7 dL / g.

3. The preparation method according to claim 1, wherein The first polyamide resin has a terminal amino group content of 40 to 50 mmol / kg and a terminal carboxyl group content of 40 to 50 mmol / kg; and / or, The second polyamide resin has a terminal amino group content of 30 to 40 mmol / kg and a terminal carboxyl group content of 30 to 40 mmol / kg.

4. The preparation method according to claim 1, wherein The mass ratio of the first polyamide resin to the second polyamide resin is 1:(0.3-0.5); and / or, In the first polyamide resin, the molar ratio of the terminal amino group to the terminal carboxyl group is 0.9 to 1.1:1; and / or, In the second polyamide resin, the molar ratio of the terminal amino group to the terminal carboxyl group is 0.9 to 1.1:1; and / or, The long carbon chain polyamide resin is a homopolymer, comprising the following structural units: Here, x is an integer selected from 9 to 11, y is an integer selected from 6 to 18, and z is an integer selected from 8 to 16.

5. The preparation method according to claim 1, wherein The long carbon chain polyamide resin is selected from PA612, PA610, PA1010, PA1012, PA1212, PA11 or PA12; and / or, The polymerization reaction temperature is 200-260° C.; and / or, The raw materials for preparing the long carbon chain polyamide resin include the first polyamide resin, the second polyamide resin, a solvent and an optional auxiliary agent; and / or, The polymerization reaction system is maintained at 200-260° C. and 1.6-2.1 MPa for 1-3 hours, and then vented and depressurized to maintain below 1000 Pa for 2-4 hours.

6. The preparation method according to claim 5, wherein: The solvent includes one or more of ethanol, methanol and water; and / or, The auxiliary agent includes an antioxidant.

7. A long carbon chain polyamide resin, prepared by the preparation method according to any one of claims 1 to 6.

8. The long carbon chain polyamide resin according to claim 7, having a viscosity of 2.4 to 2.9 dL / g; and / or, The melt strength of the long carbon chain polyamide resin is 140-210 mN.

9. A composition for preparing a long carbon chain polyamide, comprising a first polyamide resin and a second polyamide resin, wherein the first polyamide resin has a viscosity of 2.0 to 2.3 dL / g, an amino terminal content of 30 to 60 mmol / kg, and a carboxyl terminal content of 30 to 60 mmol / kg; the second polyamide resin has a viscosity of 1.5 to 1.8 dL / g, an amino terminal content of 20 to 50 mmol / kg, and a carboxyl terminal content of 20 to 50 mmol / kg.

10. The composition according to claim 9, wherein The mass ratio of the first polyamide resin to the second polyamide resin is 1:(0.3-0.5); and / or, The first polyamide resin and the second polyamide resin are of the same type and both include the following structural units: Here, x is an integer selected from 9 to 11, y is an integer selected from 6 to 18, and z is an integer selected from 8 to 16.

Citation Information

Patent Citations

  • Super-tough polyamide alloy as well as preparation method and application thereof

    CN103571178A

  • Modified polyesteramide and preparation method thereof

    CN103951822A

  • Polyamide material used for selective laser sintering and preparation method of same

    CN107286338A