Modified MOF material as well as preparation method and application thereof
By introducing defects and optimizing multi-stage pore structures of MOF materials, the modified MOF materials are formed, which solves the problems of low adsorption efficiency and insufficient site exposure, significantly improves the adsorption performance of SO2, and protects paper in the storage space of cultural relics Fiber integrity and tensile strength.
Patent Information
- Application Number
- CN202411067931.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
AI Technical Summary
When traditional MOF materials are used as adsorbents, the adsorption efficiency and insufficient exposure of adsorption sites limit their application effect in cultural relics storage space.
By introducing defects, the MOF material is modified by solvent-assisted ligand exchange method (SALE) to form a modified MOF material with a multi-stage pore structure, increasing the specific surface area and adsorption sites, and optimizing its adsorption performance on SO2.
The number of adsorption sites and the diffusion rate of gas molecules are significantly improved, efficient adsorption of SO2 is achieved, and the integrity and tensile strength of paper fibers in the storage space of cultural relics are protected.
Smart Images

Figure CN118930885A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of MOF materials, and more specifically to a modified MOF material and a preparation method and application thereof. Background Art
[0002] Cultural relics are valuable artifacts left over from the course of human history. These relics, including ancient cultural sites, tombs, ancient books, calligraphy, and paintings, represent the crystallization of humanity's great wisdom from a specific period of ancient history. Gaseous pollutants, dispersed in the atmosphere in a molecular state, can directly come into contact with cultural relics and are the most destructive factor in their destruction.
[0003] Among the many atmospheric pollutants, sulfur dioxide (SO2) is a highly active and water-soluble acidic gas that is widely distributed and highly hazardous in the atmosphere. It is also a major component of gaseous pollutants. Sulfur dioxide readily combines with atmospheric water vapor to form sulfurous acid. In the presence of metal salts, it acts as a catalyst, oxidizing sulfurous acid to sulfuric acid. When nitrogen oxides are also present in the atmosphere, SO2 reacts with substances in photochemical smog, causing a reaction. SO2 and its conversion products are highly corrosive and nonvolatile, posing a serious threat to cultural relics. Cultural relics stored in cultural relic storage spaces are constantly exposed to atmospheric pollutants, with SO2 gas being particularly damaging to fibrous, stone, leather, and metal artifacts. To protect these non-renewable cultural heritage items, the development of highly efficient adsorption materials to purify the air within these storage spaces is crucial.
[0004] At present, compared with traditional adsorbents (including zeolites and activated carbon), MOF materials have a porous crystal structure. These pores provide a large number of adsorption sites, rich metal nodes and functional adjustability, enabling MOF to be precisely designed to meet the needs of specific applications. Its adsorption mechanism mainly includes physical adsorption and chemical adsorption. The interaction of the two adsorption mechanisms enables MOF materials to achieve efficient adsorption of different gas molecules. MOF materials show great application potential due to their unique porous structure and adjustable chemical properties.
[0005] However, the single pore size of traditional MOF materials limits their adsorption performance in practical applications, resulting in problems such as low adsorption efficiency and insufficient exposure of adsorption sites. Summary of the Invention
[0006] The present invention provides a modified MOF material and a preparation method and application thereof, which are used to solve the problems in the prior art of low adsorption efficiency and insufficient exposure of adsorption sites when MOF materials are used as adsorbents.
[0007] In a first aspect, the present invention provides a modified MOF material obtained by introducing defects into a MOF material, and the modified MOF material has a multi-level pore structure.
[0008] As a possible implementation method, the MOF material is any one of UiO-66-NH2, NH2-MIL-53, MIL-101(Al)-NH2, UiO-67-NH2 and ZIF-8-NH2.
[0009] In a second aspect, the present invention provides a method for preparing a modified MOF material according to any possible implementation of the first aspect, comprising the following steps: mixing and heating the MOF material and a ligand in a solution system to obtain the modified MOF material; wherein the ratio of the MOF material to the ligand is 14 to 20 g:1 mol; and the ligand is any one of potassium sodium tartrate, terephthalic acid, and hydroxy-terephthalic acid.
[0010] As a possible implementation, the heating conditions are: temperature 50-70° C., and duration 8-12 hours.
[0011] As a possible implementation method, the MOF material is UiO-66-NH2, and the preparation method of UiO-66-NH2 includes the following steps: mixing and dissolving ZrCl4 and H2BDC-NH2 ligands in a DMF solution, adding glacial acetic acid to obtain a mixed solution; wherein, the molar ratio of ZrCl4 and H2BDC-NH2 is 1:0.8~1.2; heating the mixed solution at a temperature of 110~130°C under closed conditions for 22~26h to obtain a crude product; washing the crude product and drying it to obtain the UiO-66-NH2.
[0012] As a possible implementation manner, the crude product is washed with methanol as a washing agent; and / or the temperature for drying the crude product is 50-70°C.
[0013] In a third aspect, the present invention provides an application of the modified MOF material described in any possible implementation of the first aspect or the modified MOF material prepared by the preparation method described in any possible implementation of the second aspect in cultural relics protection.
[0014] As a possible implementation method, the modified MOF material is used to adsorb gas SO2.
[0015] As a possible implementation, the modified MOF material is used to protect the integrity of paper fibers.
[0016] UiO-66 is a Zr 4+Metal-organic frameworks (MOFs) with metal nodes have advantages such as readily available raw materials, simple synthesis, and strong corrosion resistance, and are particularly advantageous in SO2 adsorption. Their [Zr6O4(OH)4(O2C-C6H4-CO2)6] molecular configuration gives them exceptional stability in acidic and aqueous environments. UiO-66-NH2, prepared using amino-modified 2-aminoterephthalic acid as an organic ligand, exhibits both Lewis acid and alkaline properties, making it a promising catalyst for numerous acid-base combined catalytic reactions. However, while functionally group-modified UiO-66-NH2 possesses suitable adsorption sites, its microporous structure (<2.0 nm) and pore diameter (approximately 0.6 nm) hinder the exposure of active sites and inhibit the diffusion rate of gas molecules to adsorption sites within the framework. In the modified MOF material provided by the present invention, a solvent-assisted ligand exchange (SALE) method is used to cause a heterogeneous reaction between UiO-66-NH2 and potassium sodium tartrate, thereby introducing defects into UiO-66-NH2, so that some of the ligands of UiO-66-NH2 are replaced. Defects are generated inside the crystal of UiO-66-NH2, thereby forming mesopores, and obtaining a porous grade UiO-66-NH2 with a mesoporous and microporous structure, an increased specific surface area, and an enhanced adsorption capacity. In the present invention, UiO-67, ZIF-8, MIL-101 (Al) and MIL-53 can replace UiO-66 to prepare a modified MOF material with -NH2, and obtain a porous grade structure, thereby achieving the effect of increased specific surface area and enhanced adsorption capacity.
[0017] The modified MOF material provided by the present invention is regulated by the ligand, such as Figure 1 As shown, -NH2 is introduced to enhance chemical adsorption of SO2, while the multi-level pore structure is optimized to enhance physical adsorption. The team is committed to increasing the pore diameter of the material through defect engineering. On the one hand, this can expose adsorption sites within the framework, and the defect sites serve as additional adsorption sites, thereby increasing the number of available adsorption sites. On the other hand, it facilitates the diffusion of gas molecules into the framework, enhancing the mass transfer process and improving the adsorption performance of adsorbents based on ordinary MOF materials for SO2, making them more suitable for use in cultural relic storage spaces.
[0018] The multi-level porous MOF material provided by the present invention increases the number and exposure of adsorption sites while maintaining high stability, thereby improving the diffusion rate of gas molecules, thereby achieving efficient adsorption of SO2 in the storage space of cultural relics, and providing an effective environmental protection measure for the long-term preservation of cultural relics. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0020] Figure 1 Schematic diagram of the microscopic effect of the modified MOF material A provided by the present invention in adsorbing SO2 gas.
[0021] Figure 2 This is the result of the change of SO2 gas concentration at the reactor outlet over time under the action of different materials provided in the embodiment of the present invention.
[0022] Figure 3 These are the XRD and SEM analysis results of MOF material A and modified MOF material A provided in the embodiments of the present invention, wherein A is the XRD result, B and C are the SEM results of MOF material A and modified MOF material A, respectively.
[0023] Figure 4 These are SEM images of paper treated with different materials provided in the embodiments of the present invention, where A is the negative control group, B is the positive control group, C is the activated carbon group, D is the MOF material group A, and E is the modified MOF material group A. DETAILED DESCRIPTION
[0024] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0025] In order to solve the problems in the prior art of low adsorption efficiency and insufficient exposure of adsorption sites when MOF materials are used as adsorbents, the present invention provides a modified MOF material and a preparation method and application thereof.
[0026] The modified MOF material provided in the embodiment of the present invention introduces -NH2 through the regulation of ligands to enhance the chemical adsorption of SO2; and optimizes the multi-level pore structure to enhance physical adsorption. It is committed to increasing the pore diameter of UiO-66-NH2 through defect engineering. On the one hand, it can expose the adsorption sites inside the framework. The defect sites serve as additional adsorption sites, thereby increasing the number of available adsorption sites; on the other hand, it facilitates the diffusion of gas molecules into the interior of the framework, strengthens the mass transfer process, and improves the adsorption performance of the UiO-66-based adsorbent for SO2, making it better applicable to cultural relics storage spaces. When UiO-66 is replaced with UiO-67, ZIF-8, MIL-101 and MIL-53, the same effect can be achieved. The embodiment of the present invention takes UiO-66 as an example to illustrate its performance.
[0027] The embodiments of the present invention provide a preparation experiment of a MOF material and a modified MOF material, and verify their adsorption performance. It is concluded that the adsorption performance of the modified MOF material is stronger than that of the MOF material and stronger than that of the common adsorption material activated carbon.
[0028] Furthermore, the embodiments of the present invention provide application performance test experiments of MOF materials and modified MOF materials, which verify that the modified MOF materials have significant adsorption properties for SO2 gas, and can effectively improve the damage caused by SO2 gas to paper, improve the integrity of paper fibers, and enhance the tensile strength of paper.
[0029] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0030] Example 1
[0031] This embodiment provides a preparation experiment of a MOF material and a modified MOF material.
[0032] 40.0 mg of ZrCl4 (0.1716 mmol) and 31.07 mg of H2BDC-NH2 (0.1716 mmol) ligand were dissolved in 10.0 mL of DMF solution; 3.0 mL of glacial acetic acid was added to obtain a mixed solution; the mixed solution was transferred to a sealed container (a 25 mL polytetrafluoroethylene liner was used in this embodiment) and heated at 120.0°C for 24.0 h to obtain a first crude product A; the first crude product A was washed three times with methanol and dried at 60.0°C to obtain MOF material A.
[0033] 100.0 mg of MOF material A and 6.0 mmol of potassium sodium tartrate were mixed in 50.0 mL of deionized water and heated at 60° C. for 10.0 h to obtain a second crude product A; the second crude product A was washed three times with deionized water and dried at 60.0° C. to obtain a modified MOF material A.
[0034] XRD and SEM analysis were performed on MOF material A and modified MOF material A, and the following results were obtained: Figure 3 The results shown by Figure 3 It can be seen that MOF material A and modified MOF material A were successfully prepared, and defects were successfully introduced into modified MOF material A.
[0035] Example 2
[0036] This embodiment provides a preparation experiment of a MOF material and a modified MOF material.
[0037] 40.0 mg of ZrCl4 (0.1716 mmol) and 28.51 mg of 2-hydroxyterephthalic acid (H2BDC, 0.1716 mmol) ligand were dissolved in 10.0 mL of DMF solution; 3.0 mL of glacial acetic acid was added to obtain a mixed solution; the mixed solution was transferred to a sealed container (a 25 mL polytetrafluoroethylene liner was used in this embodiment) and heated at 120.0°C for 24.0 h to obtain a first crude product B; the first crude product B was washed three times with methanol and dried at 60.0°C to obtain MOF material B.
[0038] 100.0 mg of MOF material B and 6.0 mmol of hydroxyterephthalic acid were mixed in 50.0 mL of deionized water and heated at 60° C. for 10.0 h to obtain a second crude product B; the second crude product B was washed three times with deionized water and dried at 60.0° C. to obtain a modified MOF material B.
[0039] Example 3
[0040] This example provides performance testing experiments of MOF materials and modified MOF materials.
[0041] This embodiment uses a dynamic penetration test to test the material to be tested in a dynamic environment, and draws on the data testing conditions and data processing methods of activated carbon to obtain the adsorption penetration time and analyze the adsorption principle of each material.
[0042] The material to be tested was activated for 8 hours (120°C), mixed with hydroxypropyl cellulose (HPMC) in a mass ratio of 10:3, and then an appropriate amount of ethanol was added. The mixture was stirred evenly until it became a paste and heated at 50°C until the solvent was completely evaporated to obtain a MOFs / HPMC mixture. The mixture was further granulated and a 20-mesh sieve was used to sieve out the test sample with uniform particle size.
[0043] A mixed gas is obtained by mixing SO2 gas with high-purity nitrogen at a ratio of 1:2. A mass flow meter is used to accurately control the gas flow rate, with a total gas volume of 400 mL / min. A quartz tube fixed-bed reactor with an inner diameter of 16 mm and a length of 600 mm is prepared. A quartz sand core is set 300 mm from the bottom, and the sample to be tested is placed on the quartz sand core. The inlet and outlet are both covered with insulation cotton, and the outer wall is covered with an electric heating layer and a thermal insulation layer. The SO2 gas concentration is set to 300 ppm, and the total gas flow rate is 500 mL / min. A flue gas analyzer (PG-350, HORIBA) is used to monitor the changes in the SO2 concentration in the gas at the reactor outlet in real time. Breakthrough is considered when the initial concentration reaches 5%.
[0044] In this example, MOF material A, modified MOF material A, MOF material B, modified MOF material B and activated carbon prepared in Examples 1 and 2 were used as test materials to test their adsorption properties. Figure 2 The results of the change of SO2 gas concentration at the reactor outlet over time are shown.
[0045] Depend on Figure 2 As can be seen, modified MOF material A exhibits significantly stronger SO2 adsorption than MOF material A, MOF material B, modified MOF material B, and activated carbon. Modified MOF material A maintains a nearly 100% SO2 removal rate within the first 20 minutes, achieving complete SO2 penetration starting at 25 minutes and reaching complete penetration at 45 minutes, maintaining a SO2 removal rate exceeding 50% within the first 40 minutes. MOF material A's SO2 removal rate drops to approximately 40% after approximately 20 minutes, and SO2 has completely penetrated the adsorbent bed by approximately 35 minutes. Modified MOF material A exhibits significantly stronger adsorption than modified MOF material B, demonstrating that the introduction of amino groups also enhances the material's SO2 adsorption capacity. Activated carbon, a commonly used adsorbent material, is completely penetrated by SO2 after 30 minutes.
[0046] Example 4
[0047] This example provides an application performance test experiment of MOF materials and modified MOF materials.
[0048] Fill the sealed reaction chamber with SO2 gas at a concentration of 100ppm and place paper. 3 The dose of the test materials was placed in the reaction chamber and kept at a temperature of 25°C and a humidity of 50% for 260 days. A positive control group without any test materials and a negative control group in which SO2 gas was replaced by inert gas were set up. The papers in each group were characterized and analyzed by scanning electron microscopy (SEM) and the tensile strength performance test was performed.
[0049] In this example, the MOF material A, modified MOF material A, MOF material B, modified MOF material B and activated carbon prepared in Examples 1 and 2 were used as test materials to detect their effects on the integrity of paper fibers. Figure 4 The SEM results shown in Table 1 were obtained by testing the tensile strength of the paper.
[0050] Depend on Figure 4 It can be seen that the paper fiber structure in the negative control group is compact and without breakage; compared with the negative control group, the paper fiber surface in the positive control group showed obvious damage and erosion, and the structure was loose and incomplete; the integrity of the paper fiber in the activated carbon group was improved, the surface erosion was reduced, and the structure was denser; the integrity of the paper fiber in the MOF material group A was further improved, and the surface structure was better maintained; the paper fiber in the modified MOF material group A had the best integrity, the fiber structure was compact, and the degree of damage was the lowest.
[0051] Table 1 Test results of tensile strength of each group of paper
[0052] Horizontal Vertical Positive control group 0.41 0.65 Negative control group 1.2 1.91 Activated carbon group 0.63 1.12 MOF Material Group A 0.83 1.36 Modified MOF material group A 1.06 1.62 MOF Material Group B 0.78 1.18 Modified MOF material group B 0.82 1.21
[0053] Tensile strength is a key indicator of paper's toughness, reflecting the maximum torque it can withstand during stretching without breaking. Table 1 shows that, compared to the positive control group, the tensile strength of the activated carbon group increased by 62.9%, the MOF material group A increased by 105.8%, and the modified MOF material group A increased by 153.9%. The tensile strength of the modified MOF material group A was significantly greater than that of the modified MOF material group B. This indicates that the modified MOF material has significant adsorption properties for SO₂ gas and can effectively mitigate SO₂ gas damage to paper, improving the integrity of paper fibers and enhancing its tensile strength.
[0054] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0055] Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if such changes and modifications fall within the scope of the claims and their equivalents, the present invention is intended to include such changes and modifications.
Claims
1. A modified MOF material, characterized in that: The modified MOF material is obtained by introducing defects into the MOF material, and the modified MOF material has a multi-level pore structure.
2. The modified MOF material according to claim 1, characterized in that The MOF material is any one of UiO-66-NH2, UiO-67-NH2, ZIF-8-NH2, MIL-101-NH2 and NH2-MIL-53.
3. A method for preparing the modified MOF material according to any one of claims 1 to 2, characterized in that: The following steps are involved: Mixing and heating the MOF material and the ligand in a solution system to obtain the modified MOF material; The ratio of the MOF material to the ligand is 14-20 g:1 mol; the ligand is any one of potassium sodium tartrate, terephthalic acid and hydroxy-terephthalic acid.
4. The method according to claim 3, characterized in that The mixing and heating conditions are: temperature 50-70° C., and time 8-12 h.
5. The method according to claim 3, characterized in that: The MOF material is UiO-66-NH2, and the preparation method of UiO-66-NH2 comprises the following steps: Mixing and dissolving ZrCl4 and H2BDC-NH2 ligands in a DMF solution, adding glacial acetic acid to obtain a mixed solution; wherein the molar ratio of ZrCl4 to H2BDC-NH2 is 1:0.8-1.2; The mixed solution is heated at a temperature of 110 to 130° C. for 22 to 26 hours under a sealed condition to obtain a crude product; The crude product is washed and dried to obtain the UiO-66-NH2.
6. The method according to claim 5, characterized in that Washing the crude product using methanol as a washing agent; And / or, the temperature for drying the crude product is 50-70°C.
7. Use of the modified MOF material according to any one of claims 1 to 2 or the modified MOF material prepared by the preparation method according to any one of claims 3 to 6 in cultural relics protection.
8. The use according to claim 7, characterized in that: The modified MOF material is used for adsorbing gas SO2.
9. The use according to claim 7, characterized in that: The modified MOF material is used to protect the integrity of paper fibers.
Citation Information
Patent Citations
Modified metal organic framework composite material, preparation method and application
CN109438719A
Modified zirconium-based MOFs material, and preparation method and application thereof
CN110128669A
Zirconium-based organic framework compound, preparation method and applications thereof
CN111187418A
Metal-organic frameworks having localized defects for gas separations
CN114096592A
Hierarchical pore metal organic framework material as well as preparation method and application thereof