Stealth thermal protection composite material as well as preparation method and application thereof
By mixing carbon-based microwave absorbers with phenolic resin and hot-pressing, the problems of uneven dispersion and poor environmental friendliness of phenolic resin-based ablation-resistant thermal insulation composite materials have been solved, achieving both stealth and thermal protection functions, making it suitable for outer protective materials of high-speed aircraft.
Patent Information
- Application Number
- CN202411228794.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
Existing phenolic resin-based ablation-resistant thermal insulation composite materials suffer from problems such as uneven resin dispersion, high porosity, and poor environmental friendliness during the preparation process, making it difficult to achieve both stealth and thermal protection functions.
Carbon-based microwave absorbers are mixed and ground with phenolic resin, and then heat-insulating fillers are added before hot-pressing with fiber cloth. Stealth thermal protection composite materials are prepared by a one-step hot-melt method, avoiding VOC emissions and resin loss in solution impregnation. A step-curing regime with gradual temperature and pressure increases is used to control the amount of resin flowing during molding.
It achieves both radar absorption and thermal insulation functions, with good resin dispersion uniformity, high production efficiency, and controllable resin content. It is suitable for the outer protective material of high-speed aircraft and has good stealth and thermal protection performance.
Smart Images

Figure CN118930929A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wave-absorbing stealth and thermal insulation materials, and specifically relates to a stealth thermal protection composite material and a preparation method and application thereof. Background Art
[0002] With the development of aerospace technology and electronic information technology, high-speed aircraft, especially weapons and equipment, not only face the requirements of long working hours, high temperature and high pressure, but also need to have good stealth capabilities to meet the efficient strike needs of electronic information weapons and equipment.
[0003] At present, in the field of resin-based ablation-resistant thermal insulation composite materials, phenolic resin is still one of the most suitable resins for ablation-resistant thermal insulation materials because of its advantages of high cyclization rate, excellent ablation resistance, and dense and stable carbonized layer after pyrolysis. Foreign countries mainly use high-performance fibers as reinforcements to improve the mechanical, thermal stability, ablation resistance and other properties of materials, such as phenolic fiber, graphite fiber, quartz fiber, etc.; improve the heat resistance and flame retardancy of phenolic resin through chemical modification, such as boron phenolic, tungsten phenolic, phenolic cyanate, etc.; and reduce the density through physical modification by adding functional fillers to improve thermal stability, ablation rate, carbonization rate, etc., such as carbon powder, silicon carbide, etc. The composite materials used more in China are still phenolic resin / high silica glass fiber system.
[0004] Commonly used phenolic resins are usually in a plastic or rubber state at room temperature, so the current phenolic prepreg is still mainly made by solution impregnation; that is, the resin is first dissolved in an alcohol solvent according to a ratio, and the fiber reinforcement is then passed through a glue tank to absorb the resin, and the prepreg is obtained after drying. The viscosity and fluidity of the resin in this method are easy to control, but the amount of glue is difficult to accurately control. Generally, the material needs to be impregnated twice or more to ensure the uniformity of the resin distribution as much as possible; at the same time, this process consumes a large amount of volatile solvents, has poor environmental friendliness, high VOC emissions, and poor safety; in addition, as the solvent evaporates and dries, there are still problems such as large porosity and uneven product quality, so it is a production process that needs to be replaced.
[0005] Based on this, how to prepare a composite material with both stealth and thermal protection functions, ensure the dispersion and uniformity of the mixed resin, and enable large-scale and stable production, is one of the problems that need to be solved at present. Summary of the invention
[0006] The purpose of the present invention is to provide a stealth thermal protection composite material and a preparation method and application thereof. The stealth thermal protection composite material has both radar absorbing stealth and heat insulation protection effects, and at the same time has good raw material dispersion and coating uniformity, and strong controllability and laying operability.
[0007] The technical solution adopted to achieve the above purpose is to provide a method for preparing a stealth thermal protection composite material, comprising the following steps:
[0008] (1) mixing a carbon-based absorber and a phenolic resin, stirring and grinding the mixture to obtain a mixed resin I;
[0009] (2) adding a heat-insulating filler to the mixed resin I and stirring at the same temperature to obtain a mixed resin II;
[0010] (3) coating the mixed resin II on the release paper, and then covering the surface of the mixed resin II with fiber cloth and hot pressing and impregnating it to obtain a prepreg;
[0011] (4) Cutting the prepreg and laying it in a mold and hot pressing and curing it to obtain a stealth thermal protection composite material.
[0012] The beneficial effects of the technical solution of the present invention are as follows: in the present invention, the carbon absorber is first mixed with the phenolic resin. Since the carbon absorber has high surface energy, is easy to agglomerate and has strong oil absorption, it needs to be fully dispersed in the resin by strong force. Therefore, it is first necessary to stir and then grind. The stirring and grinding process ensures the uniform dispersion of the absorber in the resin, avoiding uneven performance caused by excessively high or low local concentrations. In order to avoid the hollow thermal insulation filler from being squeezed and broken during the dispersion process, thereby losing the thermal insulation and density properties, the thermal insulation filler needs to be ground evenly before the carbon absorber and the phenolic resin are ground. Add; then cover the surface of the mixed resin II with fiber cloth and hot press impregnate. In order to ensure that the carbon absorber and thermal insulation filler are fully dispersed in the resin and have good coating properties, the phenolic resin used needs to have a low viscosity, and phenolic resin is a self-polymerizing resin, which means that the average molecular weight of the resin is also low at low viscosity. In order to ensure the film-forming property of the resin on the prepreg and the operability of the prepreg ply, the phenolic resin needs to be prepolymerized in the hot press impregnation stage to reach a certain degree of reaction, ensure good bonding between the fiber cloth and the resin, and show appropriate viscosity to facilitate subsequent ply curing operations.
[0013] Preferably, the carbon absorber is at least one of graphene, carbon nanotubes, carbon black and silicon carbide; the phenolic resin is aminophenolic resin, bariumphenolic resin or boronphenolic resin; the thermal insulation filler is hollow phenolic microspheres or hollow glass microspheres; and the fiber cloth is quartz fiber cloth or high silica glass fiber cloth.
[0014] The beneficial effects of the above technical solution adopted in the present invention are as follows: graphene, carbon nanotubes, carbon black and silicon carbide are carbon-based absorbers with low density, all of which have good electromagnetic wave absorption ability and can effectively reduce the reflection of electromagnetic waves such as radar waves, thereby enhancing the stealth performance of the composite material. Graphene and carbon nanotubes can achieve efficient electromagnetic wave absorption at a lower content due to their unique nanostructure and excellent conductivity, while maintaining the lightweight characteristics of the material, while carbon black and silicon carbide provide a lasting stealth effect in the composite material due to their stable chemical properties and good dispersibility; aminophenol-formaldehyde resin has good water resistance and chemical corrosion resistance. Barium phenolic resin and boron phenolic resin have higher heat resistance and flame retardancy due to the introduction of barium or boron elements, which helps to improve the thermal protection performance of the composite material. The hollow structure of hollow phenolic microspheres or hollow glass microspheres can make them have lower density and thermal conductivity, which can effectively block the transfer of heat and improve the thermal insulation performance of the composite material. The hollow phenolic microspheres have better compatibility with the phenolic resin matrix, which may help to improve the overall strength and stability of the composite material. The hollow glass microspheres are suitable for thermal protection applications in high temperature environments due to their good chemical stability and high temperature resistance.
[0015] More preferably, the phenolic resin is barium phenolic resin; and the fiber cloth is quartz fiber cloth.
[0016] The beneficial effects of the technical solution adopted in the present invention are as follows: the barium phenolic resin has low viscosity, good ablation resistance and high cost performance; the quartz fiber cloth has higher SiO2 purity, smaller linear expansion coefficient and better heat resistance stability.
[0017] More preferably, the graphene has a conductivity of 1000 to 50000 S / m, a particle size of 1 to 100 μm, and a specific surface area of 100 to 300 m 2 / g and bulk density is 0.01~0.05g / cm 3 The reduced graphene oxide powder; the carbon nanotube has a diameter of 5 to 20 nm, a length of 50 to 500 μm, and a specific surface area of 200 to 400 m 2 / g and bulk density is 0.05~0.3g / cm 3 The carbon black has a resistivity of 0.1 to 1 Ω·m, a particle size of 5 to 20 μm, and a specific surface area of 500 to 1000 m 2 / g of conductive carbon black; the phenolic resin is a solvent-free phenolic resin, the solvent-free phenolic resin has a solid content of>90wt%, a residual carbon rate of>60% and a viscosity of 500-10000cP / 50°C; the particle size of the thermal insulation filler is 10-100μm / D50, and the density is 0.2-0.6g / cm 3 The compressive strength is 3-60MPa; the fiber surface density of the fiber cloth is 50-500g / m 2 .
[0018] More preferably, the graphene has a conductivity of 5000 to 10000 S / m, a particle size of 10 to 20 μm, and a specific surface area of 200 to 250 m 2 / g and bulk density is 0.02~0.04g / cm 3 The reduced graphene oxide powder; the carbon nanotube has a diameter of 10-15 nm, a length of 50-100 μm, and a specific surface area of 250-300 m 2 / g and bulk density is 0.1~0.2g / cm 3 The carbon black has a resistivity of 0.5 to 0.8 Ω·m, a particle size of 10 to 15 μm and a specific surface area of 600 to 800 m 2 / g of conductive carbon black; solvent-free phenolic resin with a solid content of 95-98wt%, a residual carbon rate of 70-80% and a viscosity of 500-2000cP / 50°C; a particle size of the thermal insulation filler of 10-100μm / D50 and a density of 0.2-0.6g / cm 3 The compressive strength is 3-60MPa; the fiber surface density of the fiber cloth is 100-300g / m 2 .
[0019] More preferably, the fiber weaving form of the fiber cloth includes plain weave, twill weave or satin weave.
[0020] Preferably, the mass ratio of the carbon absorber, the phenolic resin, the thermal insulation filler and the fiber cloth is (0.2-5):(37.5-57.5):(10-20):(20-40).
[0021] Preferably, the stirring in step (1) is mechanical stirring, the stirring speed is 100-1000 r / min, the time is 10-60 min, and the temperature is 25-35° C.; the grinding is performed using a three-roll grinder, the roller gap is 0.01-0.1 mm, the single grinding time is 0.5-6 h, the number of grindings is 3-10 times, and the temperature is 35-45° C.; after grinding, the mixed resin I scraper fineness meter test is <20 μm.
[0022] More preferably, in step (1), the stirring speed is 300-500 r / min, and the time is 20-30 min; a three-roll grinder is used for grinding, the roller gap is 0.01-0.03 mm, the single grinding time is 1-2 h, and the number of grinding times is 5-6 times.
[0023] Preferably, the heat preservation stirring in step (2) is mechanical stirring, the stirring speed is 100-500 r / min, the heat preservation temperature is 40-70° C., and the stirring time is 10-50 min.
[0024] More preferably, in step (2), the speed of the heat preservation stirring is 200 to 300 r / min, the heat preservation temperature is 50 to 65° C., and the stirring time is 20 to 50 min.
[0025] Preferably, the coating in step (3) is single-sided coating or double-sided coating, and the coating amount is 100 to 500 g / m 2 The glue coating temperature is 30-80°C, the glue coating speed is 1-10m / min; the hot pressing impregnation temperature is 100-150°C, the hot pressing pressure is 0.2-0.5MPa, the length of the impregnation section drying tunnel is 20-50m, and the impregnation time is 5-20min.
[0026] More preferably, the coating in step (3) is double-sided adhesive coating.
[0027] More preferably, the coating temperature in step (3) is 60-75° C., and the coating speed is 2-5 m / min.
[0028] More preferably, the hot press impregnation temperature is 110 to 135°C.
[0029] More preferably, after hot pressing and impregnation in step (3), the upper release paper is peeled off and a PE mesh film is laid, the exhaust passage is maintained, and the film is rolled up for standby use to obtain a prepreg.
[0030] More preferably, in step (4), the thickness of the prepreg is 0.4 to 1.0 mm, and the number of prepreg sheets is >10.
[0031] Preferably, the hot pressing curing molding in step (4) adopts a hot pressing tank molding process, with a temperature of 60 to 180° C., a pressure of 1 to 10 bar, and a time of 2 to 20 hours.
[0032] More preferably, the hot pressing curing molding in step (4) adopts a step-by-step curing system in which the temperature and pressure of the autoclave are gradually increased.
[0033] More preferably, the step-by-step curing system of gradually increasing the temperature and pressure of the autoclave is: curing at 60°C and 1 bar for 1 hour, then curing at 80°C and 3 bar for 1 hour, then curing at 100°C and 5 bar for 2 hours, then curing at 130°C and 7 bar for 2 hours, and finally curing at 170°C and 9 bar for 3 hours.
[0034] The beneficial effect of the technical solution adopted in the present invention is that the step-by-step curing system of gradually increasing temperature and pressure can make the resin experience different temperature and pressure steps, thereby controlling the molding glue flow and achieving sufficient exhaust, reducing product defects and improving the yield rate.
[0035] The present invention also provides a stealth thermal protection composite material prepared by the above preparation method.
[0036] The present invention also provides the use of the stealth thermal protection composite material in preparing the outer protective material of a high-speed aircraft.
[0037] The present invention has the following beneficial effects:
[0038] (1) In the stealth thermal protection composite material prepared by the present invention, phenolic resin, carbon-based absorber and thermal insulation filler are first mixed and reacted to make it have both thermal insulation protection and wave absorbing stealth functions; the prepreg obtained by compounding it with fiber cloth can be used to prepare the outer protective cover of high-speed aircraft, thereby realizing a composite structure with normalized stealth and thermal protection functions.
[0039] (2) The prepreg production process of the present invention is a one-step direct hot melt method, which avoids the problems of high VOC emission and poor prepreg uniformity in the production of phenolic prepreg by the traditional solution impregnation method, and also avoids the problems of large auxiliary material consumption and resin loss in the two-step film calendering method. It also has the advantages of precise control of resin content and high production efficiency.
[0040] (3) The raw material content of the stealth thermal protection composite material of the present invention can be flexibly adjusted within a certain range, so that a series of prepregs with functional differences can be produced according to actual needs, and can be switched relatively quickly on the production line, thereby being able to prepare functionally graded composite structures to meet application requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a schematic diagram of the prepreg composition structure of the stealth thermal protection composite material;
[0042] Figure 2 This is a schematic diagram of the structure of the stealth thermal protection composite material in Example 2;
[0043] Among them, 1. phenolic resin matrix; 2. fiber cloth reinforcement; 3. thermal insulation filler; 4. carbon absorber; 5. composite material layer with 0.2wt% carbon absorber content; 6. composite material layer with 0.5wt% carbon absorber content; 7. composite material layer with 1wt% carbon absorber content; 8. composite material layer with 2wt% carbon absorber content; 9. composite material layer with 5wt% carbon absorber content. DETAILED DESCRIPTION
[0044] The features and performance of the present invention are further described in detail below in conjunction with embodiments.
[0045] Example 1
[0046] A method for preparing a stealth thermal protection composite material comprises the following steps:
[0047] (1) Reduced graphene oxide powder, barium phenolic resin, hollow glass microspheres and quartz fiber cloth were weighed in a mass ratio of 2.5:47.5:10:40; wherein the reduced graphene oxide powder had an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3 ; Barium phenolic resin solid content 97wt%, residual carbon rate 72% and viscosity 550cP / 50℃, gel time 495s / 130℃; hollow glass microsphere particle size 60μm / D50, microsphere density 0.25g / cm 3 , compressive strength 5MPa; quartz fiber cloth has a fiber surface density of 200g / m 2 Plain D-type quartz fiber cloth;
[0048] (2) Mixing the reduced graphene oxide powder and the barium phenolic resin at 25° C. with a paddle-type mechanical stirring at a speed of 500 r / min for 20 min, and then grinding 5 times at 35° C. with a three-roll mill with a roller gap of 0.015 mm, each grinding for 1.5 h, to obtain a mixed resin I. The mixed resin I was tested by a scraper fineness meter and was <20 μm;
[0049] (3) adding the hollow glass microspheres to the mixed resin I and stirring at 55° C. and 300 r / min for 30 min to obtain a mixed resin II;
[0050] (4) Coat the mixed resin II on the release paper by double-sided gluing, with a coating amount of 300g / m 2 , the gluing temperature is 65°C, the gluing speed is 3m / min, and then the surface of the mixed resin II is covered with quartz fiber cloth, the quartz fiber cloth is located in the middle of the mixed resin II on both sides of the upper and lower release papers, and hot pressing and impregnation at 125°C are performed. The pressure of the roller during hot pressing is 0.3MPa, the length of the impregnation section drying tunnel is 30m, and the impregnation time is 10min. After hot pressing and impregnation, the upper release paper is peeled off and the PE grid film is laid, the exhaust passage is maintained, and the prepreg with a single layer thickness of 0.55±0.02mm is obtained;
[0051] (5) 20 prepreg sheets are cut into a size of 300 mm*300 mm and layered in a mold in sequence. After layering, they are wrapped in a vacuum bag and equipped with a vacuum valve and sent into an autoclave for hot pressing and curing. The hot pressing and curing adopts a step-by-step curing system in which the temperature and pressure of the autoclave are gradually increased: curing at 60°C and 1 bar for 1 hour, then curing at 80°C and 3 bar for 1 hour, then curing at 100°C and 5 bar for 2 hours, then curing at 130°C and 7 bar for 2 hours, and finally curing at 170°C and 9 bar for 3 hours to obtain a stealth thermal protection composite material.
[0052] In this embodiment, the prepreg composition structure is as follows Figure 1 shown.
[0053] Example 2
[0054] A method for preparing a stealth thermal protection composite material comprises the following steps:
[0055] (1) Reduced graphene oxide powder, barium phenolic resin, hollow glass microspheres and quartz fiber cloth were weighed in a mass ratio of 0.2:49.8:10:40, 0.5:49.5:10:40, 1:49:10:40, 2:48:10:40 and 5:45:10:40 respectively for use; wherein the reduced graphene oxide powder has an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3 ; Barium phenolic resin solid content 97wt%, residual carbon rate 72% and viscosity 550cP / 50℃, gel time 495s / 130℃; hollow glass microsphere particle size 60μm / D50, microsphere density 0.25g / cm 3 , compressive strength 5MPa; quartz fiber cloth has a fiber surface density of 200g / m 2 Plain D-type quartz fiber cloth;
[0056] (2) Reduced graphene oxide powder and barium phenolic resin in different mass ratios were mixed at 25°C and stirred at a speed of 500 r / min for 20 min with a paddle type mechanical stirring, and then ground five times at 35°C using a three-roll mill with a roller gap of 0.015 mm, each grinding for 1.5 h, to obtain mixed resins I-1, I-2, I-3, I-4 and I-5 with reduced graphene oxide powder contents from low to high, respectively. The scraper fineness test results of mixed resins I-1 to 5 were all <20 μm;
[0057] (3) adding the hollow glass microspheres to the mixed resins I-1 to 5 respectively, and stirring at 55° C. and 300 r / min for 30 min to obtain mixed resins II-1 to 5;
[0058] (4) The mixed resins II-1 to II-5 were coated on the release paper by double-sided gluing, and the coating amount was 300 g / m 2, the gluing temperature is 65℃, the gluing speed is 3m / min, and then the surfaces of the mixed resins II-1~5 are covered with quartz fiber cloth respectively, the quartz fiber cloth is located in the middle of the mixed resin II on both sides of each upper and lower release paper, and hot pressing and impregnation at 125℃ are performed. The pressure of the roller during hot pressing is 0.3MPa, the length of the impregnation section drying tunnel is 30m, and the impregnation time is 10min. After hot pressing and impregnation, the upper release paper is peeled off and the PE grid film is laid, the exhaust passage is maintained, and the prepregs 1~5 with a single layer thickness of (0.5~0.6)±0.02mm are obtained;
[0059] (5) Prepregs 1 to 5 are cut into a size of 300 mm*300 mm and layered in a mold in sequence. Four pieces of prepreg 1, prepreg 2, prepreg 3, prepreg 4 and prepreg 5 are layered in sequence from outside to inside. After layering, they are wrapped in a vacuum bag and equipped with a vacuum valve and sent into an autoclave for hot pressing and curing. The hot pressing and curing adopts a step-by-step curing system in which the temperature and pressure of the autoclave are gradually increased: curing at 60°C and 1 bar for 1 hour, then curing at 80°C and 3 bar for 1 hour, then curing at 100°C and 5 bar for 2 hours, then curing at 130°C and 7 bar for 2 hours, and finally curing at 170°C and 9 bar for 3 hours to obtain a stealth thermal protection composite material.
[0060] In this embodiment, the stealth thermal protection composite material structure is as follows Figure 2 shown.
[0061] Example 3
[0062] A method for preparing a stealth thermal protection composite material comprises the following steps:
[0063] (1) Weighing an absorber, barium phenolic resin, hollow glass microspheres and quartz fiber cloth in a mass ratio of 2.5:47.5:10:40; wherein the absorber comprises reduced graphene oxide powder, multi-walled carbon nanotubes and conductive carbon black in a mass ratio of 2:0.4:0.1, and the reduced graphene oxide powder has an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3 The diameter of the multi-walled carbon nanotube is 10nm, the length is 100μm, and the specific surface area is 250m 2 / g and bulk density 0.1g / cm 3 The conductive carbon black has a resistivity of 0.8Ω·m, a particle size of 12μm and a specific surface area of 600m 2 / g; barium phenolic resin solid content 97wt%, residual carbon rate 72% and viscosity 550cP / 50℃, gel time 495s / 130℃; hollow glass microsphere particle size 60μm / D50, microsphere density 0.25g / cm 3, compressive strength 5MPa; quartz fiber cloth has a fiber surface density of 200g / m 2 Plain D-type quartz fiber cloth;
[0064] (2) adding conductive carbon black, multi-walled carbon nanotubes and reduced graphene oxide powder to barium phenolic resin in sequence, mixing at 25° C. and stirring with a paddle type mechanical stirring at a speed of 500 r / min for 20 min, and then grinding 5 times at 35° C. using a three-roll mill with a roller gap of 0.015 mm, each grinding for 1.5 h, to obtain a mixed resin I, and the mixed resin I was tested by a scraper fineness meter with a value of <20 μm;
[0065] (3) adding the hollow glass microspheres to the mixed resin I and stirring at 55° C. and 300 r / min for 30 min to obtain a mixed resin II;
[0066] (4) Coat the mixed resin II on the release paper by double-sided gluing, with a coating amount of 300g / m 2 , the gluing temperature is 65°C, the gluing speed is 3m / min, and then the surface of the mixed resin II is covered with quartz fiber cloth, the quartz fiber cloth is located in the middle of the mixed resin II on both sides of the upper and lower release papers, and hot pressing and impregnation at 125°C are performed. The pressure of the roller during hot pressing is 0.3MPa, the length of the impregnation section drying tunnel is 30m, and the impregnation time is 10min. After hot pressing and impregnation, the upper release paper is peeled off and the PE grid film is laid, the exhaust passage is maintained, and the prepreg with a single layer thickness of 0.56±0.02mm is obtained;
[0067] (5) 20 prepreg sheets are cut into a size of 300 mm*300 mm and layered in a mold in sequence. After layering, they are wrapped in a vacuum bag and equipped with a vacuum valve and sent into an autoclave for hot pressing and curing. The hot pressing and curing adopts a step-by-step curing system in which the temperature and pressure of the autoclave are gradually increased: curing at 60°C and 1 bar for 1 hour, then curing at 80°C and 3 bar for 1 hour, then curing at 100°C and 5 bar for 2 hours, then curing at 130°C and 7 bar for 2 hours, and finally curing at 170°C and 9 bar for 3 hours to obtain a stealth thermal protection composite material.
[0068] Example 4
[0069] A method for preparing a stealth thermal protection composite material comprises the following steps:
[0070] (1) Reduced graphene oxide powder, barium phenolic resin, hollow glass microspheres and quartz fiber cloth were weighed in a mass ratio of 2.5:37.5:20:40; wherein the reduced graphene oxide powder had an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3; Barium phenolic resin solid content 97wt%, residual carbon rate 72% and viscosity 550cP / 50℃, gel time 495s / 130℃; hollow glass microsphere particle size 60μm / D50, microsphere density 0.2g / cm 3 , compressive strength 3.5MPa; quartz fiber cloth has a fiber surface density of 200g / m 2 Plain D-type quartz fiber cloth;
[0071] (2) Mixing the reduced graphene oxide powder and the barium phenolic resin at 25° C. with a paddle-type mechanical stirring at a speed of 500 r / min for 20 min, and then grinding 5 times at 35° C. with a three-roll mill with a roller gap of 0.015 mm, each grinding for 1.5 h, to obtain a mixed resin I. The mixed resin I was tested by a scraper fineness meter and was <20 μm;
[0072] (3) adding the hollow glass microspheres to the mixed resin I and stirring at 65° C. and 300 r / min for 40 min to obtain a mixed resin II;
[0073] (4) Coat the mixed resin II on the release paper by double-sided gluing, with a coating amount of 300g / m 2 , the gluing temperature is 75°C, the gluing speed is 5m / min, and then the surface of the mixed resin II is covered with quartz fiber cloth, the quartz fiber cloth is located in the middle of the mixed resin II on both sides of the upper and lower release papers, and hot pressing and impregnation at 135°C are performed. The pressure of the roller during hot pressing is 0.3MPa, the length of the impregnation section drying tunnel is 30m, and the impregnation time is 6min. After hot pressing and impregnation, the upper release paper is peeled off and the PE grid film is laid, the exhaust passage is maintained, and the prepreg with a single layer thickness of 0.82±0.03mm is obtained;
[0074] (5) 14 prepreg sheets are cut into a size of 300 mm*300 mm and layered in a mold in sequence. After layering, they are wrapped in a vacuum bag and equipped with a vacuum valve and sent into an autoclave for hot pressing and curing. The hot pressing and curing adopts a step-by-step curing system in which the temperature and pressure of the autoclave are gradually increased: curing at 60°C and 1 bar for 1 hour, then curing at 80°C and 3 bar for 1 hour, then curing at 100°C and 5 bar for 2 hours, then curing at 130°C and 7 bar for 2 hours, and finally curing at 170°C and 9 bar for 3 hours to obtain a stealth thermal protection composite material.
[0075] Example 5
[0076] A method for preparing a stealth thermal protection composite material comprises the following steps:
[0077] (1) Reduced graphene oxide powder, barium phenolic resin, hollow glass microspheres and quartz fiber cloth were weighed in a mass ratio of 2.5:57.5:20:20; wherein the reduced graphene oxide powder had an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3 ; Barium phenolic resin solid content 97wt%, residual carbon rate 72% and viscosity 550cP / 50℃, gel time 495s / 130℃; hollow glass microsphere particle size 60μm / D50, microsphere density 0.2g / cm 3 , compressive strength 3.5MPa; quartz fiber cloth has a fiber surface density of 100g / m 2 Plain C-shaped quartz fiber cloth;
[0078] (2) Mixing the reduced graphene oxide powder and the barium phenolic resin at 25° C. with a paddle-type mechanical stirring at a speed of 500 r / min for 20 min, and then grinding 5 times at 35° C. with a three-roll mill with a roller gap of 0.015 mm, each grinding for 1.5 h, to obtain a mixed resin I. The mixed resin I was tested by a scraper fineness meter and was <20 μm;
[0079] (3) adding the hollow glass microspheres to the mixed resin I and stirring at 65° C. and 200 r / min for 50 min to obtain a mixed resin II;
[0080] (4) Coat the mixed resin II on the release paper by double-sided gluing, with a coating amount of 400g / m 2 , the gluing temperature is 75°C, the gluing speed is 5m / min, and then the surface of the mixed resin II is covered with quartz fiber cloth, the quartz fiber cloth is located in the middle of the mixed resin II on both sides of the upper and lower release papers, and hot pressing and impregnation are performed at 130°C. The pressure of the roller during hot pressing is 0.2MPa, the length of the impregnation section drying tunnel is 30m, and the impregnation time is 6min. After hot pressing and impregnation, the upper release paper is peeled off and the PE mesh film is laid, the exhaust passage is maintained, and the prepreg with a single layer thickness of 0.85±0.03mm is obtained;
[0081] (5) 13 pieces of prepreg are cut into a size of 300 mm*300 mm and layered in a mold in sequence. After layering, they are wrapped in a vacuum bag and equipped with a vacuum valve and sent into an autoclave for hot pressing and curing. The hot pressing and curing adopts a step-by-step curing system in which the temperature and pressure of the autoclave are gradually increased: curing at 60°C and 1 bar for 1 hour, then curing at 80°C and 3 bar for 1 hour, then curing at 100°C and 5 bar for 2 hours, then curing at 130°C and 7 bar for 2 hours, and finally curing at 170°C and 9 bar for 3 hours to obtain a stealth thermal protection composite material.
[0082] Example 6
[0083] A method for preparing a stealth thermal protection composite material comprises the following steps:
[0084] (1) Reduced graphene oxide powder, barium phenolic resin, hollow phenolic microspheres and quartz fiber cloth were weighed in a mass ratio of 2.5:47.5:10:40; wherein the reduced graphene oxide powder had an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3 The solid content of barium phenolic resin is 97wt%, the residual carbon rate is 72%, the viscosity is 550cP / 50℃, and the gel time is 495s / 130℃; the particle size of hollow phenolic microspheres is 65μm / D50, and the density of microspheres is 0.2g / cm 3 , compressive strength 4.5MPa; quartz fiber cloth has a fiber surface density of 200g / m 2 Plain D-type quartz fiber cloth;
[0085] (2) Mixing the reduced graphene oxide powder and the barium phenolic resin at 25° C. with a paddle-type mechanical stirring at a speed of 500 r / min for 20 min, and then grinding 5 times at 35° C. with a three-roll mill with a roller gap of 0.015 mm, each grinding for 1.5 h, to obtain a mixed resin I. The mixed resin I was tested by a scraper fineness meter and was <20 μm;
[0086] (3) adding the hollow phenolic microspheres to the mixed resin I and stirring at 60° C. and 300 r / min for 30 min to obtain a mixed resin II;
[0087] (4) Coat the mixed resin II on the release paper by double-sided gluing, with a coating amount of 300g / m 2 , the gluing temperature is 70°C, the gluing speed is 4m / min, and then the surface of the mixed resin II is covered with quartz fiber cloth, the quartz fiber cloth is located in the middle of the mixed resin II on both sides of the upper and lower release papers, and hot pressing and impregnation at 130°C are performed. The pressure of the roller during hot pressing is 0.3MPa, the length of the impregnation section drying tunnel is 30m, and the impregnation time is 7.5min. After hot pressing and impregnation, the upper release paper is peeled off and the PE grid film is laid, the exhaust passage is maintained, and the prepreg with a single layer thickness of 0.60±0.02mm is obtained;
[0088] (5) 18 pieces of prepreg are cut into a size of 300 mm*300 mm and layered in a mold in sequence. After layering, they are wrapped with a vacuum bag and equipped with a vacuum valve and sent into an autoclave for hot pressing and curing. The hot pressing and curing adopts a step-by-step curing system in which the temperature and pressure of the autoclave are gradually increased: curing at 60°C and 1 bar for 1 hour, then curing at 80°C and 3 bar for 1 hour, then curing at 100°C and 5 bar for 2 hours, then curing at 130°C and 7 bar for 2 hours, and finally curing at 170°C and 9 bar for 3 hours to obtain a stealth thermal protection composite material.
[0089] Comparative Example 1
[0090] A method for preparing a mixed resin material comprises the following steps:
[0091] (1) Reduced graphene oxide powder and barium phenolic resin were weighed in a mass ratio of 2.5:47.5; wherein the reduced graphene oxide powder had an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3 ; Barium phenolic resin has a solid content of 98wt%, a residual carbon rate of 73%, a viscosity of 15500cP / 50℃, and a gel time of 430s / 130℃;
[0092] (2) The reduced graphene oxide powder and the barium phenolic resin were mixed at 25° C. and stirred at a speed of 300 r / min for 20 min with a paddle type mechanical stirring, and then ground three times at 40° C. using a three-roll mill with a roller gap of 0.020 mm, each grinding for 5 h, to obtain a mixed resin I. The mixed resin I was tested by a scraper fineness meter and was <30 μm.
[0093] The phenolic resin used in this comparative example has a very high viscosity and is difficult to stir mechanically. The prepared mixed resin I cannot be added with thermal insulation fillers, and the preparation of the stealth thermal protection composite material cannot be completed.
[0094] Comparative Example 2
[0095] A method for preparing a stealth thermal protection composite material comprises the following steps:
[0096] (1) Reduced graphene oxide powder, barium phenolic resin, hollow glass microspheres and quartz fiber cloth were weighed in a mass ratio of 2.5:47.5:10:40; wherein the reduced graphene oxide powder had an electrical conductivity of 8500 S / m, a particle size of 15 μm, and a specific surface area of 240 m 2 / g and bulk density is 0.025g / cm 3; Barium phenolic resin solid content 97wt%, residual carbon rate 72% and viscosity 550cP / 50℃, gel time 495s / 130℃; hollow glass microsphere particle size 60μm / D50, microsphere density 0.25g / cm 3 , compressive strength 5MPa; quartz fiber cloth has a fiber surface density of 200g / m 2 Plain D-type quartz fiber cloth;
[0097] (2) Mixing the reduced graphene oxide powder and the barium phenolic resin at 25° C. with a paddle-type mechanical stirring at a speed of 500 r / min for 20 min, and then grinding 5 times at 35° C. with a three-roll mill with a roller gap of 0.015 mm, each grinding for 1.5 h, to obtain a mixed resin I. The mixed resin I was tested by a scraper fineness meter and was <20 μm;
[0098] (3) adding the hollow glass microspheres to the mixed resin I and stirring at 55° C. and 300 r / min for 30 min to obtain a mixed resin II;
[0099] (4) Coat the mixed resin II on the release paper by double-sided gluing, with a coating amount of 300g / m 2 , the gluing temperature is 65°C, the gluing speed is 3m / min, and then the surface of the mixed resin II is covered with quartz fiber cloth, the quartz fiber cloth is located in the middle of the mixed resin II on both sides of the upper and lower release papers, and hot pressing and impregnation at 125°C are performed. The pressure of the roller during hot pressing is 0.3MPa, the length of the impregnation section drying tunnel is 30m, and the impregnation time is 10min. After hot pressing and impregnation, the upper release paper is peeled off and the PE grid film is laid, the exhaust passage is maintained, and the prepreg with a single layer thickness of 0.55±0.02mm is obtained;
[0100] (5) 20 prepreg sheets are cut into a size of 300 mm*300 mm and layered in a mold in sequence. After layering, they are wrapped in a vacuum bag and equipped with a vacuum valve and sent into an autoclave for hot pressing and curing. The hot pressing and curing adopts a one-step curing system of the autoclave: curing for 8 hours at 130°C and 6 bar to obtain a stealth thermal protection composite material.
[0101] During the preparation process of the stealth thermal protection composite material in this comparative example, the glue flow of the cured sample reached 12%, and multiple delamination gaps appeared inside the sample, indicating that the curing system did not match and the quality of the obtained stealth thermal protection composite material product was unqualified.
[0102] Experimental example
[0103] The bow method of the national military standard GJB2038A-2011 was used to test the wave absorption performance of the stealth thermal protection composite material prepared in Examples 1 to 3 of the present invention. The composite material was trimmed into the size of the test sample according to the test requirements, assembled on the device, and the reflection loss was measured in the frequency range of 2 to 18 GHz to characterize the wave absorption performance. The test results are shown in Table 1.
[0104] Table 1 Wave absorbing properties of stealth thermal protection composite materials
[0105]
[0106] In this embodiment, GJB330A-2000 and GB / T22588-2008 are used to test the specific heat capacity and thermal conductivity of the stealth thermal protection composite materials prepared in Examples 1 to 2 and 4 to 6 of the present invention. According to the test requirements, the composite materials are cut into the size of the tested samples, assembled into the device, tested at a specified temperature, and GJB323A-1996 is used to test the mass ablation rate and the line ablation rate. The test results are shown in Table 2.
[0107] Table 2 Thermal insulation and ablation resistance of stealth thermal protection composite materials
[0108]
[0109]
[0110] It can be seen from Tables 1 to 2 that by changing the content of the absorber and different gradient combinations, the effective absorption bandwidth of the composite material structure can be expanded, and the absorbing efficiency of the composite material structure can be improved; with the increase of the content of thermal insulation filler, the ablation resistance of the composite material structure is improved; the proportion and type of each component of the resin, absorber, thermal insulation filler and fiber cloth in the prepreg can be adjusted according to the actual application requirements. The stealth thermal protection composite material prepared by the present invention has good absorbing stealth effect and thermal protection effect, good overall dispersion and coating uniformity, the resin content of the prepreg is controllable and the layering operability is strong during the preparation process, and the composite material has good molding processability.
[0111] The present invention has been described according to the above embodiments. It should be understood that the above embodiments do not limit the present invention in any form. Any technical solutions obtained by equivalent replacement or equivalent transformation shall fall within the scope of the present invention.
Claims
1. A method for preparing a stealth thermal protection composite material, characterized in that: The following steps are involved: (1) mixing a carbon-based absorber and a phenolic resin, stirring and grinding the mixture to obtain a mixed resin I; (2) adding a heat-insulating filler to the mixed resin I and stirring at the same temperature to obtain a mixed resin II; (3) coating the mixed resin II on the release paper, and then covering the surface of the mixed resin II with fiber cloth and hot pressing and impregnating it to obtain a prepreg; (4) Cutting the prepreg and laying it in a mold and hot pressing and curing it to obtain a stealth thermal protection composite material.
2. The method for preparing the stealth thermal protection composite material according to claim 1, characterized in that: The carbon-based absorber is at least one of graphene, carbon nanotubes, carbon black and silicon carbide; the phenolic resin is aminophenolic resin, bariumphenolic resin or boronphenolic resin; the thermal insulation filler is hollow phenolic microspheres or hollow glass microspheres; the fiber cloth is quartz fiber cloth or high-silica glass fiber cloth.
3. The method for preparing the stealth thermal protection composite material according to claim 2, characterized in that: The graphene has a conductivity of 1000 to 50000 S / m, a particle size of 1 to 100 μm, and a specific surface area of 100 to 300 m 2 / g and bulk density is 0.01~0.05g / cm 3 The reduced graphene oxide powder; the carbon nanotubes have a diameter of 5 to 20 nm, a length of 50 to 500 μm, and a specific surface area of 200 to 400 m 2 / g and bulk density is 0.05~0.3g / cm 3 The carbon black has a resistivity of 0.1 to 1Ω·m, a particle size of 5 to 20μm and a specific surface area of 500 to 1000m 2 / g of conductive carbon black; the phenolic resin is a solvent-free phenolic resin, the solvent-free phenolic resin has a solid content of>90wt%, a residual carbon rate of>60% and a viscosity of 500-10000cP / 50°C; the particle size of the thermal insulation filler is 10-100μm / D50, and the density is 0.2-0.6g / cm 3 The compressive strength is 3-60 MPa; the fiber surface density of the fiber cloth is 50-500 g / m 2 .
4. The method for preparing the stealth thermal protection composite material according to claim 1, characterized in that: The mass ratio of the carbon-based absorber, phenolic resin, thermal insulation filler and fiber cloth is (0.2-5):(37.5-57.5):(10-20):(20-40).
5. The method for preparing the stealth thermal protection composite material according to claim 1, characterized in that: The stirring in step (1) is mechanical stirring, the stirring speed is 100-1000 r / min, the time is 10-60 min, and the temperature is 25-35° C.; the grinding is performed using a three-roll grinder, the roller gap is 0.01-0.1 mm, the single grinding time is 0.5-6 h, the number of grindings is 3-10 times, and the temperature is 35-45° C.; after the grinding, the mixed resin I scraper fineness meter test is <20 μm.
6. The method for preparing the stealth thermal protection composite material according to claim 1, characterized in that: In the step (2), the heat preservation stirring is mechanical stirring, the stirring speed is 100-500 r / min, the heat preservation temperature is 40-70° C., and the stirring time is 10-50 min.
7. The method for preparing the stealth thermal protection composite material according to claim 1, characterized in that: The coating in step (3) is single-sided or double-sided coating, and the coating amount is 100 to 500 g / m 2 The glue coating temperature is 30-80°C, and the glue coating speed is 1-10m / min; the hot pressing impregnation temperature is 100-150°C, the hot pressing pressure is 0.2-0.5MPa, the impregnation section drying tunnel length is 20-50m, and the impregnation time is 5-20min.
8. The method for preparing the stealth thermal protection composite material according to claim 1, characterized in that: The hot pressing curing molding in step (4) adopts a hot pressing tank molding process, with a temperature of 60 to 180° C., a pressure of 1 to 10 bar, and a time of 2 to 20 hours.
9. A stealth thermal protection composite material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the stealth thermal protection composite material according to claim 9 in the preparation of outer protective materials for high-speed aircraft.