Additive containing phosphite ester and amino siloxane, anti-ionizing radiation aromatic polyester material and preparation method of anti-ionizing radiation aromatic polyester material

By introducing alkyl phosphites and aminosiloxanes as radiation-resistant additives into aromatic polyester materials, the problems of easy embrittlement and yellowing of traditional aromatic polyester materials under high-energy radiation are solved, and the performance of the materials in high-radiation environments is improved.

CN118930973APending Publication Date: 2024-11-12JIANGSU TONGWEI XINDA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028072.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional aromatic polyester materials are prone to radiation yellowing and radiation embrittlement under high-energy electromagnetic waves or high-energy ion current radiation. Existing anti-radiation additives cannot effectively solve this problem and may even aggravate radiation yellowing.

Method used

A radiation-resistant additive system without aromatic units, comprising alkyl phosphites and aminosiloxanes, is used in aromatic polyester materials to form ionizing radiation-resistant composite materials through compounding and granulation.

Benefits of technology

To prevent radiation-induced yellowing under high radiation doses, improve the mechanical rigidity and toughness of materials, maintain the overall performance of materials, and make them suitable for high-radiation environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an additive containing phosphite ester and amino siloxane, an anti-ionizing radiation aromatic polyester material and a preparation method of the anti-ionizing radiation aromatic polyester material. Mixing alkyl phosphite and amino siloxane to obtain an anti-radiation additive, uniformly stirring and mixing the additive with the properly dried aromatic polyester master batch, and uniformly mixing the master batch mixed with the additive; finally, the blended material is granulated again to serve as the ionizing radiation resistant aromatic polyester modified master batch, and the master batch can be used independently or blended with other plastics according to needs. The molecular chemical structure of the additive formula does not contain aromatic hydrocarbon groups such as benzene rings, so that the problems of radiation yellowing and high toxicity of the traditional aromatic hydrocarbon anti-radiation agent are fundamentally avoided. The additive formula is small in volatility, air pollution in the processing process can be reduced, meanwhile, radiation curing embrittlement caused by excessive radiation self-crosslinking and benzene ring rigidity of aromatic polyester can be remarkably relieved, and the anti-radiation requirements for keeping rigidity and toughness of aromatic polyester under the scene of high ionizing radiation dose are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of radiation-resistant modification of materials, and in particular to an additive containing phosphite and aminosiloxane, an aromatic polyester material resistant to ionizing radiation, and a preparation method thereof. Background Art

[0002] When plastics and other organic polymers are exposed to ionizing radiation such as high-energy electromagnetic waves, high-energy ion currents, and high-energy electron beams, the original molecular chains will be broken by high-energy impacts, forming free radicals or ionized fragment end groups. Then, these broken chain links tend to be mainly radiolytic or mainly cross-linked, depending on the chemical structure properties. In most cases, the continuous accumulation of high radiation doses will eventually cause the overall polymer material to tend to be radiolytic, showing adverse consequences such as radiation embrittlement and radiation yellowing of the material on a macro scale. At present, the widely used radiation disinfection of imported and exported goods, radiation sterilization of medical supplies, and nuclear power plant cable equipment all encounter the ionizing radiation hazards of plastics and other polymer parts or packaging materials. Therefore, the development of radiation-resistant formulas for plastics and other polymer materials has practical significance and economic value.

[0003] Aromatic polyesters are a common class of materials in general-purpose plastics. They mainly tend to crosslink under ionizing radiation. However, due to the rigidity of the benzene ring units, excessive self-crosslinking caused by radiation makes this type of material face the problem of radiation embrittlement. Traditional benzene-containing anti-radiation additives cannot overcome this contradiction, but instead aggravate the radiation yellowing caused by the presence of aromatic units in the additives.

[0004] Based on this, the present invention provides an anti-radiation additive formulation system which does not contain aromatic units, has a molecular structure mainly composed of fully saturated CC or CO units, and has long-chain alkyl or alkoxy units with soft chain segments. Summary of the invention

[0005] The present invention aims to provide a fully saturated chain, high boiling point, easy-to-mix anti-radiation additive system to address the shortcomings of common aromatic anti-radiation agents that are prone to radiation yellowing and radiation embrittlement under high ionizing radiation doses. Compared with other traditional anti-radiation formulations, this formulation system does not have the disadvantage of radiation yellowing, and can maintain or even improve the mechanical rigidity and toughness of aromatic polyester materials under radiation doses of several hundred kGy.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0007] An additive is applicable to a formulation system of aromatic polyester for resisting ionizing radiation, and the additive comprises alkyl phosphite and aminosiloxane.

[0008] As a possible implementation mode, further, the aromatic polyester is a polycarboxylate containing a benzene ring functional group structure, such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polybutylene terephthalate adipate (PBAT) and other polyesters containing aromatic hydrocarbon structures.

[0009] As a possible implementation manner, further, the alkyl phosphite is a phosphite compound whose side group contains only saturated alkyl groups and whose alkyl carbon chain length is more than four carbon atoms, such as triisooctyl phosphite, triisodecyl phosphite, etc.

[0010] As a possible implementation mode, further, the aminosiloxane is an organic silicon compound having a fully saturated molecular chain, an amino group at one end of the molecule and an alkoxy silicon structure at the other end, such as 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, etc.

[0011] The invention also provides an aromatic polyester material resistant to ionizing radiation, comprising aromatic polyester and the above additive.

[0012] As a possible implementation manner, further, the amount of the alkyl phosphite added is 0.1% to 10% relative to the total weight of the raw materials; the amount of the aminosiloxane added is 0.1% to 10% relative to the total weight of the raw materials.

[0013] Furthermore, the additive molecular structure does not contain aromatic structures or unsaturated olefin units; the ionizing radiation-resistant aromatic polyester material can withstand processing temperatures below 300 degrees.

[0014] The present invention provides a method for preparing the above-mentioned aromatic polyester material resistant to ionizing radiation, characterized in that it comprises the following steps:

[0015] 1) Pre-drying the aromatic polyester raw material for standby use;

[0016] 2) adding alkyl phosphite and aminosiloxane to the dried pure aromatic polyester raw material and stirring and mixing;

[0017] 3) adding the mixed material to a melting device such as an internal mixer or a screw extruder, and mixing it at the internal mixing temperature of the pure raw material of the aromatic polyester to be processed until it is uniform;

[0018] 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain an aromatic polyester modified masterbatch.

[0019] As a possible implementation, further, in step 2), the alkyl phosphite and the aminosiloxane are added separately to the pure aromatic polyester raw material, or the alkyl phosphite and the aminosiloxane are pre-mixed and then added to the pure aromatic polyester raw material.

[0020] As a possible implementation method, further, the additives in an amount less than 3-5% can be added to the aromatic polyester raw material at one time for mixing, and the excess amount of the additives needs to be added gradually in the subsequent mixing and kneading process.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0022] 1) The molecular chemical structure of the aromatic polyester material additive formula provided by the present invention does not contain aromatic hydrocarbon groups such as benzene rings, which fundamentally avoids the problems of radiation yellowing and high toxicity of traditional aromatic hydrocarbon anti-radiation agents.

[0023] 2) The additive formula of the present invention has low volatility and can reduce air pollution during the processing process. At the same time, it can significantly alleviate the radiation curing brittleness of aromatic polyesters caused by excessive radiation self-crosslinking and benzene ring rigidity, and can maintain or even improve the mechanical rigidity and toughness of aromatic polyester materials under a radiation dose of several hundred kGy, taking into account the radiation resistance requirements of aromatic polyesters in terms of rigidity and toughness under high ionizing radiation dose scenarios, and has excellent industrial application prospects. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The present invention provides an additive, an aromatic polyester material resistant to ionizing radiation and a preparation method thereof, wherein the aromatic polyester material resistant to ionizing radiation comprises an additive suitable for an aromatic polyester anti-ionizing radiation formulation system and an aromatic polyester; wherein the aromatic polyester is any polycarboxylate containing a benzene ring functional group structure, such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polybutylene terephthalate adipate (PBAT) and other polyesters containing aromatic hydrocarbon structures.

[0026] Additives suitable for aromatic polyester anti-ionizing radiation formulation systems include alkyl phosphites and aminosiloxanes. Among them, alkyl phosphites are phosphite compounds in which any side group contains only saturated alkyl groups and the length of the alkyl carbon chain is more than four carbon atoms, such as triisooctyl phosphite and triisodecyl phosphite; aminosiloxanes are organic silicon compounds in which any molecular chain is a fully saturated bond and one end of the molecule contains an amine group and the other end contains an alkoxy silicon structure, such as 3-aminopropyl triethoxysilane, N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, etc.

[0027] The molecular structure of the above-mentioned additive does not contain any aromatic structure or any unsaturated olefin unit. According to the specific ingredients of the formula, it can withstand processing temperatures such as mixing or injection molding below 300 degrees.

[0028] The preparation method of the aromatic polyester material resistant to ionizing radiation specifically comprises the following steps:

[0029] 1) The aromatic polyester raw material is first dried in a drying equipment such as a blast dryer at 60-90°C for 1-4 hours for use. If it is not used immediately after drying, the polyester raw material is sealed in a dry state at 30-40°C. If it is stored openly, it needs to be dried again before use;

[0030] 2) Add the additives in a weight percentage relative to the total feed, wherein the addition amount of alkyl phosphite is 0.1% to 10%, and the addition amount of aminosiloxane is 0.1% to 10%; mix the additives with the polyester pellets dried in the above step 1) and stir evenly, alkyl phosphite and aminosiloxane can be added to the pure aromatic polyester raw material separately, or alkyl phosphite and aminosiloxane can be pre-mixed and then added to the pure aromatic polyester raw material. Additives less than about 3% to 5% can be mixed at one time, and the excess additives need to be added gradually during the subsequent mixing and kneading process.

[0031] 3) The mixed material in the above step 2) is put into a mixing equipment such as an internal mixer for internal mixing. The internal mixing temperature is set to the melting temperature of the aromatic pure raw material. The internal mixing time is 5 to 30 minutes, during which the remaining additives can be added successively.

[0032] 4) The raw materials after mixing are taken out and crushed by a plastic crusher and other equipment, and then re-granulated to obtain the final granular radiation-resistant composite material, which can be used as the masterbatch of various plastic products for anti-ionizing radiation purposes. It has good anti-ionizing radiation performance and can be used alone or blended with other plastics.

[0033] Example 1

[0034] Take 98% of PBAT (polybutylene terephthalate adipate) masterbatch (weight percentage relative to the total feed, the following percentages of ingredients have the same meaning), dry it in a blast dryer at 80 degrees for 2 hours, cool it to 30-40 degrees and take it out. Mix two additives: 1% triisobutyl phosphite and 1% N-(2-aminoethyl)-3-aminopropyl trimethoxysilane with the dried PBAT masterbatch. Then put the mixture into a mixer and mix it at 150℃ for 8 minutes. After the mixing is completed, take it out and put it into a plastic crusher for crushing. Put the crushed mixture into a twin-screw extruder for re-granulation. The temperature of each zone of the extruder is 130-145℃ and the speed is 50-60r / min.

[0035] The radiation-resistant composite masterbatch finally obtained in this embodiment was injected into a dumbbell-shaped mechanical test sample to test the change of the formula on the radiation resistance of the polyester masterbatch. The test conditions were: the electron accelerator energy was 10 MeV, the temperature was room temperature (25°C), and the ambient atmosphere was exposed to ordinary air. The radiation resistance of the sample is as follows:

[0036] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the pure PBAT sample in the non-added group increases from about 22 MPa before irradiation to 23.5 MPa after irradiation (self-crosslinking by bulk radiation); but the tensile elongation at break decreases from about 700% before irradiation to about 630% after irradiation (radiation embrittlement); the tensile strength of the composite sample of the present embodiment increases from 24 MPa before irradiation to 26.5 MPa after irradiation, and the elongation at break increases from about 640% before irradiation to about 660% after irradiation (radiation toughening).

[0037] When the electron beam radiation dose increases from 0 kGy to 300 kGy, the tensile strength of the pure PBAT sample in the non-added group increases from 22 MPa to 23 MPa (bulk radiation self-crosslinking), but the tensile elongation at break decreases from about 700% to about 560% (radiation embrittlement); the sample of the composite material of this embodiment increases from 24 MPa to about 27 MPa, and the elongation at break increases from about 640% to 690% (radiation toughening).

[0038] This compounding ratio achieves the goal of keeping the PBAT polyester material in this example within the range of high radiation doses below 300 kGy, while simultaneously increasing the radiation-resistant rigidity (tensile strength) and toughness (elongation at break) of the sample.

[0039] Example 2

[0040] The preparation process of the radiation-resistant composite material is the same as that in Example 1, and PBAT polyester is still used as the bulk masterbatch, but the ratio is different. PBAT is taken at 98.9%, and the additive formula ratio is changed to: 1% N-(2-aminoethyl)-3-aminopropyltrimethoxysilane is added, and 0.1% triisobutyl phosphite is added. The same electron beam irradiation conditions as in Example 1 are adopted.

[0041] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the composite sample with this ratio increases from 25.5 MPa to 29 MPa, and the tensile elongation at break increases from 630% to 660%.

[0042] When the electron beam radiation dose increases from 0 kGy to 300 kGy, the tensile strength of the composite sample with this ratio increases from 25.5 MPa to 26.5 MPa, and the tensile elongation at break decreases from 630% to 600%;

[0043] This compounding ratio significantly enhances the radiation-resistant rigidity (tensile strength) and radiation-resistant toughness (elongation at break) of the sample at a moderate radiation dose of about 100 kGy, and at the same time slightly alleviates the radiation embrittlement of the PBAT polyester material at a high radiation dose (such as 300 kGy in this example) after addition.

[0044] Example 3

[0045] The preparation process of the radiation-resistant composite material is the same as that in Example 1, and PBAT polyester is still used as the main masterbatch, but the ratio is different. PBAT is taken at 98.9%, and the additive formula ratio is changed to: N-(2-aminoethyl)-3-aminopropyltrimethoxysilane is added at 0.1%, and triisobutyl phosphite is added at 1%. The same electron beam irradiation conditions as in Example 1 are adopted.

[0046] When the electron beam radiation dose increases from 0kGy to 100kGy, the tensile strength of the composite sample with this ratio remains unchanged at 23Mpa, and the tensile elongation at break increases from 670% to 710%;

[0047] When the electron beam radiation dose increases from 0kGy to 300kGy, the tensile strength of the composite sample with this ratio remains almost unchanged at 23Mpa, and the tensile elongation at break increases from 670% to 750%;

[0048] This compounding ratio keeps the radiation-resistant rigidity of the composite sample almost unchanged within the experimental high radiation dose range (below 300 kGy), and its outstanding feature is that it can greatly improve the radiation-resistant toughness (tensile elongation at break) of the composite sample within the high radiation dose range.

[0049] In summary, for the two types of additives involved in the present invention, for the polyester masterbatch PBAT, the main function of triisobutyl phosphite is radiation toughening, and the main function of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane is radiation enhancement. The focus of additive feeding can be adjusted for different aromatic polyester masterbatches according to actual needs.

[0050] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An additive, characterized in that: The additive is suitable for the formulation system of aromatic polyester to resist ionizing radiation, and comprises alkyl phosphite and aminosiloxane.

2. The additive according to claim 1, characterized in that The aromatic polyester is a polycarboxylate containing a benzene ring functional group structure.

3. The additive according to claim 1, characterized in that The alkyl phosphite is a phosphite compound in which the side groups only contain saturated alkyl groups and the length of the alkyl carbon chain is more than four carbon atoms.

4. The additive according to claim 1, characterized in that The aminosiloxane is an organic silicon compound with a fully saturated bond in the molecular chain, an amino group at one end of the molecule and an alkoxy silicon structure at the other end.

5. An aromatic polyester material resistant to ionizing radiation, characterized in that: The invention comprises an aromatic polyester and the additive according to any one of claims 1 to 4.

6. The ionizing radiation resistant aromatic polyester material according to claim 5, characterized in that: The addition amount of the alkyl phosphite is 0.1% to 10% relative to the total weight of the raw materials; the addition amount of the aminosiloxane is 0.1% to 10% relative to the total weight of the raw materials.

7. The ionizing radiation resistant aromatic polyester material according to claim 5, characterized in that: The additive molecular structure does not contain aromatic hydrocarbon structure and unsaturated olefin unit; the ionizing radiation resistant aromatic polyester material can withstand processing temperatures below 300 degrees.

8. A method for preparing an aromatic polyester material resistant to ionizing radiation according to any one of claims 5 to 7, characterized in that: The steps include: 1) Pre-drying the aromatic polyester raw material for standby use; 2) adding alkyl phosphite and aminosiloxane to the dried pure aromatic polyester raw material and stirring and mixing; 3) Add the mixed material to the melting equipment to be processed into 10000 pure raw materials of aromatic polyester Mix at the internal mixing temperature until uniform; 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain an aromatic polyester modified masterbatch.

9. The method for preparing the ionizing radiation resistant aromatic polyester material according to claim 8, characterized in that: In step 2), the alkyl phosphite and the aminosiloxane are added to the pure aromatic polyester raw material separately, or the alkyl phosphite and the aminosiloxane are pre-mixed and then added to the pure aromatic polyester raw material.

10. The method for preparing the ionizing radiation resistant aromatic polyester material according to claim 8, characterized in that: The additives in an amount less than 3-5% can be added to the aromatic polyester raw material at one time for mixing, and the excess amount of additives needs to be added gradually in the subsequent mixing and kneading process.