Preparation method of hollow glass bead / rubber composite material

By performing double modification and wet kneading process of silane coupling agent and polymer on the surface of hollow glass microbeads, the poor mechanical properties and microbead crushing problems of the existing medium and low-density rubber materials are solved, and lightweight and high The preparation of strong rubber composite materials improves the compatibility and mechanical properties of the materials.

CN118931051APending Publication Date: 2024-11-12HENAN UNIVERSITY +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411173599.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the preparation of low-density rubber materials, the mechanical properties are reduced by foaming methods, and the foaming equipment is large in investment and complex in process. The unmodified hollow glass microbeads have poor compatibility with rubber, which are easy to break, affecting the material performance. .

Method used

By double modification of the surface of hollow glass microbeads by silane coupling agent and polymer, it improves its compatibility with rubber and interface interaction, and uses wet kneading to reduce shear force, protect the microbead structure, and spray drying Enhance the interface bonding force and prepare lightweight, high-strength rubber composite materials.

Benefits of technology

Effectively improve the compatibility between hollow glass microbeads and rubber, reduce rubber density, improve the mechanical properties of composite materials, simplify processes, and has the potential for large-scale production. The material density does not exceed 0.83 g/cm3, and the tensile strength reaches 2.0 MPa or above. , the elongation rate of break is above 350%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a preparation method of a hollow glass bead / rubber composite material. The preparation method comprises the following steps: activating and modifying the surfaces of hollow glass beads; and carrying out wet-process mixing and vulcanization with rubber to obtain the low-density rubber composite material. According to the method, the preparation process is simple, the compatibility between the modified glass beads and a rubber matrix is obviously improved, the density of the prepared bead / rubber composite material is obviously reduced, and meanwhile, good tensile strength and fracture strain performance are maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of materials, and particularly relates to a method for preparing a low-density hollow glass microsphere / rubber composite material by using double-layer surface-modified hollow glass microspheres as fillers through a wet mixing method. Background Art

[0002] As a commonly used high-elastic polymer, rubber has good insulation, sealing, weather resistance and mechanical properties, so it can be widely used in various fields. With the development of social science and technology and economy, the application scope of rubber has been further expanded, and more special requirements have been put forward for it. For example, in the fields of aerospace, drones, and new energy vehicles, rubber is required to have good mechanical properties and a low density, which can not only increase the load of aircraft or automobiles and improve the mass ratio, but also effectively reduce fuel consumption; in the civilian range, such as shoe materials, vulcanized rubber retains good elasticity and wear resistance while reducing rubber density, which can significantly improve wearing comfort. In the process of preparing low-density rubber, foaming is a more commonly used lightweight means, and the thermal insulation performance of the material can be improved by foaming and pore formation. But at the same time, it will also significantly affect the mechanical properties of rubber. In addition, the investment in foaming equipment is large, the production process is complex, and chemical foaming will also pollute the environment. On the other hand, by adjusting the ingredients of the rubber formula and adding effective lightweight fillers, it has become an effective way to prepare low-density rubber materials.

[0003] Hollow glass microspheres are thin-walled and lightweight (density between 0.1 and 1.0 g.cm -3 ) and is often used as a lightweight filler in rubber matrix. Its main component is borosilicate, with a particle size distribution range of 10 to 250 μm and a wall thickness of 1 to 2 μm. It has the characteristics of low density, heat insulation, high compressive strength, good fluidity and stability. In the preparation process of hollow glass microsphere / rubber composite materials, the raw rubber is usually mixed with each component additive and filler by an open mixer and an internal mixer. In this process, the high viscosity of the raw rubber and the multiple extrusion and stirring processes will exert excessive shear force on the hollow glass microspheres, inevitably causing the microspheres to break. In addition, the unmodified hollow glass microspheres have poor compatibility with rubber, and their interfacial interaction is weak. The microspheres are easily detached from the rubber matrix, forming defects in the composite material, which greatly reduces the mechanical properties of the rubber.

[0004] Based on this, this application was developed. Summary of the invention

[0005] The present invention aims to overcome the defects of the prior art and provide a method for preparing a hollow glass microsphere / rubber composite material, aiming to provide a lightweight, high-strength rubber composite material. The surface of the hollow glass microsphere is double-modified by a silane coupling agent and a polymer, which can improve the compatibility and interface interaction with the hollow glass microsphere and form a stable chemical bond. The wet mixing preparation method can achieve mixing of the hollow glass microsphere and the rubber at a low shear strength, thereby protecting the structural integrity of the hollow glass microsphere.

[0006] To achieve the above object, the present invention adopts the following technical solutions: A method for preparing a hollow glass microsphere / rubber composite material comprises the following steps: (1) Surface activation of hollow glass microspheres: a certain mass of hollow glass microspheres is added to an alkaline aqueous solution of a certain concentration, stirred and reacted at 25-60°C for 0.5-3h, and then filtered and washed to obtain activated hollow glass microspheres; then the activated hollow glass microspheres are added with water to prepare an aqueous dispersion of a certain concentration; (2) Modifying hollow glass microspheres with silane coupling agent: adding a certain amount of silane coupling agent to the aqueous dispersion prepared in step (1), adjusting the pH to 7.5-10.5, heating to 50-60°C for reaction for 0.5-2h, and then heating to 60-100°C for reaction for 2-4h to graft the silane coupling agent onto the surface of the hollow glass microspheres, thereby obtaining a hollow glass microsphere dispersion modified with a silane coupling agent; (3) Polymer-modified hollow glass microspheres: Weigh a certain amount of polymer and dissolve it in water, add it to the silane coupling agent-modified hollow glass microsphere dispersion obtained in step (2), adjust the pH to 6-9, and react at 20-90° C. for 0.5-2 h (the polymer is coated on the surface of the hollow glass microspheres by heating and sufficient stirring), to obtain a polymer-modified hollow glass microsphere dispersion; (4) spray drying: spray drying the polymer-modified hollow glass microsphere dispersion of step (3) to obtain surface-modified hollow glass microsphere powder; (5) Wet mixing of hollow glass microsphere / rubber composite: Add the rubber additive dispersion except the vulcanizer and the surface modified hollow glass microsphere powder dispersion to the rubber dispersion or oil-based solution, disperse them evenly, and obtain the mixed rubber after flocculation precipitation or heating to remove the solvent. Then add the vulcanizer on the open mill, and then vulcanize to obtain the hollow glass microsphere / rubber composite material (low-density rubber composite material). The true density of the hollow glass microsphere is less than 0.6g / cm 3 , D90 particle size is less than 80μm, and compressive strength is less than 26000psi.

[0007] Specifically, in step (1), the mass percentage concentration of the alkaline aqueous solution is 0.1 to 20%; the alkali can be an inorganic base or an organic base, including but not limited to one or more inorganic bases such as sodium hydroxide, potassium hydroxide, sodium bicarbonate, and organic bases such as tetramethylammonium hydroxide and tetrabutylammonium hydroxide.

[0008] Furthermore, in step (1), the pH value of the final washing solution is within the range of 7 to 9, and the mass percentage of the activated hollow glass microspheres in the redispersed aqueous dispersion is within the range of 1 to 20%.

[0009] Specifically, in step (2), the silane coupling agent may be an alkoxysilane coupling agent, a silazane coupling agent, or a silicone oil, including but not limited to alkoxy coupling agents such as bis-[γ-(triethoxysilyl)propyl] tetrasulfide, 3-glycidyloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, dimethyldiethoxysilane, and vinyltrimethoxysilane, silazane coupling agents such as hexamethyldisilazane, and silicone oils such as hydroxy silicone oil, hydrogenated silicone oil, and vinyl silicone oil. The amount of the silane coupling agent used may be 0.1% to 20% of the mass of the hollow glass microspheres after activation in step (1).

[0010] Specifically, in step (3), the polymer may include, but is not limited to, hydrophilic polymers such as polyethylene glycol, polyvinyl alcohol, polyacrylic acid, polyvinyl pyrrolidone, hydrolyzed maleic anhydride, polyvinyl acetate, ethylene-vinyl acetate copolymer, or one or more of water-based rubber latex such as natural rubber, latex polystyrene butadiene rubber latex, nitrile latex, chloroprene rubber latex, bio-based itaconate rubber, or oil-based rubber solution such as solution polystyrene butadiene rubber, EPDM rubber, butadiene rubber, etc. The amount of polymer used is 1 to 20% of the mass of the activated hollow glass microspheres in step (1). When the hollow glass microspheres are modified with a polymer, it is preferred to first use sulfuric acid to adjust the pH range to 6 to 9, and then add the polymer. The polymer can be coated on the surface of the hollow glass microspheres by heating and sufficient stirring (such as ultrasonic stirring for 0.5 to 2 hours).

[0011] Furthermore, in step (4), the inlet temperature of the spray drying is 200-350°C, the outlet temperature is 80-110°C, and the feed speed is 30-60 rpm.

[0012] Specifically, in step (5), the rubber additives include one or more of demulsifiers, accelerators, vulcanizers, vulcanization activators, antioxidants, softeners, etc.; wherein the demulsifiers include but are not limited to one or more of acids such as formic acid, acetic acid or salts such as zinc sulfate, calcium chloride, magnesium chloride, sodium chloride, etc.; the accelerators include one or more of accelerators CZ, accelerator D, accelerator DM, accelerator TMTD, etc.; the vulcanizers include one or two of sulfur, diisopropylbenzene peroxide DCP, 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane, 2,4-dichloroperoxybenzoyl, etc.; the vulcanization activators include one or more of sulfur, diisopropylbenzene peroxide DCP, 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane, 2,4-dichloroperoxybenzoyl, etc. Including but not limited to one or more of zinc stearate, stearic acid, zinc oxide, etc.; the softener includes one or more of paraffin, microcrystalline wax, cyclohexane oil, coumarone resin, etc.; in the rubber additives, the amount of demulsifier is 0-20 parts by weight, the amount of accelerator is 0.5-5 parts by weight, the amount of vulcanizer is 0.5-5 parts by weight, the amount of vulcanizing agent is 1-5 parts by weight, the amount of antioxidant is 1-2 parts by weight, and the amount of softener is 1-2 parts; except for the demulsifier, it is dispersed in water or organic solvent in proportion to prepare a rubber additive dispersion with a mass concentration of 10-40%; the demulsifier is separately prepared into a 1-20% solution.

[0013] Furthermore, the surface modified hollow glass microsphere powder is used in an amount of 5 to 60 parts by weight and is prepared into a water or organic dispersion with a mass concentration of 15 to 50%.

[0014] Furthermore, the rubber may be selected from natural rubber and / or synthetic rubber, including but not limited to one or more of natural rubber, emulsion-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, nitrile rubber, butadiene rubber, ethylene propylene diene rubber, bio-based itaconate rubber, etc.; the rubber is formulated into an aqueous dispersion or dissolved in an organic solvent to prepare a rubber oil-based solution, and the mass concentration of the rubber is 1 to 60% based on 100 parts by weight of the rubber dry rubber.

[0015] Preferably, when one or more water-based rubber latexes such as natural rubber, latex polystyrene butadiene rubber, bio-based itaconate, etc. are used, a dispersion of rubber additives other than a vulcanizer is poured into the rubber latex, and after high-speed shear dispersion for 0.5 to 2 hours, an aqueous dispersion of surface-modified hollow glass microbeads is added, and the speed is reduced and stirred and dispersed for 0.5 to 2 hours, and finally a demulsifier solution is added for flocculation and precipitation, and filtered, and the solid wet mixed rubber material is taken out and dried to obtain a mixed rubber; When one or more of oil-based rubbers including but not limited to solution-polymerized styrene-butadiene rubber, nitrile rubber, butadiene rubber, ethylene-propylene-diene rubber and the like are used, a dispersion of rubber additives other than a vulcanizing agent is poured into a rubber solution, and after high-speed shearing dispersion for 0.5 to 2 hours, an organic dispersion of surface-modified hollow glass microspheres is added, and the dispersion is stirred and dispersed at a reduced speed for 0.5 to 2 hours, followed by reduced-pressure distillation to recover the organic solvent, and the solid wet-mixed rubber material is taken out and dried to obtain a mixed rubber; Finally, a vulcanizing agent is added to the mixed rubber on an open mixing mill, and then vulcanization is carried out (vulcanization temperature is 150-180° C., and vulcanization pressure is 5-20 MPa) to obtain a hollow glass microsphere / rubber composite material.

[0016] The present application provides a method for preparing a hollow glass microsphere / rubber composite material. The surface activation of the hollow microspheres enhances the activity of the surface hydroxyl groups, which is conducive to forming a stable chemical bond with the subsequent silane coupling agent. By modifying the first layer of silane coupling agent on the surface of the hollow glass microspheres, the number of hydroxyl groups on the surface of the microspheres is reduced, the affinity of the microspheres for organophilicity is improved, and the presence of short-chain molecules forms a barrier effect, reducing the agglomeration between the hollow glass microspheres. By coating the surface with a second layer of polymer, the surface polarity of the hollow glass microspheres is more matched with the rubber matrix, the interfacial bonding force between the glass microspheres and the rubber matrix is ​​effectively enhanced, and an effective transition layer is formed between the glass microspheres and the rubber matrix; and the polymer coating can protect the microspheres during the mixing process, effectively disperse the shear force on the surface of the microspheres, thereby reducing the breakage rate of the microspheres during the mixing process. At the same time, the spray drying process promotes the dehydration condensation between the surface of the hollow microspheres-silane coupling agent, silane coupling agent-polymer, polymer-hollow glass microspheres, and the surface hydroxyl groups, thereby improving the interfacial bonding force between the polymer and the hollow glass microspheres to ensure the stable coating of the polymer during the subsequent wet mixing process. In addition, in the existing mixing technology for preparing hollow glass microspheres / rubber materials, the high-intensity shear force generated during the commonly used banburying, open mixing, and hot pressing processes can easily cause the hollow glass microspheres to break. Compared with the prior art, the wet mixing preparation method provided by the present application, in which the hollow glass microspheres are added to the liquid phase rubber solution, can effectively reduce the shear force during the mixing process and avoid the large-scale breakage of the hollow glass microspheres. The method of the present invention can not only effectively improve the compatibility of the hollow glass microspheres with rubber, reduce the rubber density, but also improve the mechanical properties of the hollow glass microspheres / rubber lightweight composite material. Moreover, the process of the method is simple and has the potential for large-scale production.

[0017] Compared with the prior art, the method of double-layer surface modified hollow glass microspheres of the present invention has the following advantages and beneficial effects: 1) The present invention increases the active sites on the surface of the glass hollow microspheres and improves the grafting rate of the silane coupling agent and the polymer by alkali activation of the glass hollow microspheres; 2) The present invention modifies the glass microspheres with a silane coupling agent to improve the organophilicity of the microspheres, and at the same time grafts a macromolecular polymer on the surface thereof to enhance the compatibility and contact area with the rubber matrix, and forms a polymer transition layer between the microspheres and the rubber substrate to disperse the shear force received during the mixing process; 3) The present invention spray-dries the modified hollow glass microspheres, utilizes instantaneous high temperature to promote the coating of the polymer on the surface of the glass microspheres, controls the particle size, and reduces the adhesion between the microspheres; 4) The wet mixing preparation method proposed in the present invention disperses the corresponding fillers and processing aids in a solvent and mixes them with the rubber solution, thereby reducing the shear force on the hollow glass microspheres during the mixing process, thereby reducing their breakage rate and further improving the dispersibility of the hollow glass microspheres in the colloid, thereby achieving the performance requirements of the rubber composite material in terms of lightweight and high strength; 5) The hollow glass microsphere / rubber material prepared by the present invention has a density of no more than 0.83 g / cm3, a tensile strength of more than 2.0 MPa, and an elongation at break of more than 350%. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The double-layer modified hollow glass microspheres in Example 3; Figure 2 This is a cross-sectional electron microscope scanning image of the surface-modified hollow glass microsphere / rubber material in Example 3; After the surface modification, the bonding strength between the hollow glass microspheres and the rubber substrate is enhanced. After the rubber composite material is brittle fractured by liquid nitrogen, it can be observed on its cross section that most of the double-layer surface-modified hollow glass microspheres are half-embedded in the rubber substrate and will not fall off with the fracture of the rubber substrate. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is further described in detail below in conjunction with the embodiments, but the protection scope of the present invention is not limited thereto.

[0020] The raw materials used in the examples are all commercially available products that can be directly purchased or prepared by conventional methods in the art. For example, the hollow glass microspheres are from Zhengzhou Shenglait Hollow Microsphere New Materials Co., Ltd., and the true density of the hollow glass microspheres is less than 0.6 g / cm 3 , D90 particle size is less than 80μm, and compressive strength is less than 26000psi.

[0021] Example 1 A method for preparing a hollow glass microsphere / rubber composite material comprises the following steps: (1) Prepare 250 mL of 1% tetramethylammonium hydroxide aqueous solution, add 25 g of hollow glass microspheres with a particle size of 30 μm, stir at 60°C for 30 minutes, filter and wash the hollow glass microspheres with deionized water until the pH value of the filtrate stabilizes at 8-9, and obtain activated hollow glass microspheres; (2) adding deionized water to the hollow glass microspheres activated in step (1) to prepare a 10% aqueous dispersion by mass, stirring to uniformly disperse the hollow glass microspheres in the water; adding 0.5 g of γ-aminopropyltriethoxysilane and 0.7 g of aqueous ammonia to adjust the pH value of the dispersion to 9, heating to 60° C. and keeping the temperature constant for 1 hour; then heating to 80° C. and keeping the temperature constant for 2 hours to obtain a silane coupling agent-modified hollow glass microsphere dispersion; (3) adding 1 g of a 10% sulfuric acid solution to the reaction system of step (2), adjusting the pH value of the dispersion to 6, and then adding 5 g of a 10% polyvinyl alcohol aqueous solution, stirring at room temperature 25° C. for 1 hour to disperse uniformly, to obtain a polymer-modified hollow glass microsphere dispersion; (4) spray drying the dispersion obtained in step (3), setting the spray drying inlet temperature to 250° C., the outlet temperature to 100° C., and the feed rate to 30 rpm, to obtain a final double-layer modified hollow glass microsphere product; (5) EPDM rubber (100 phr): 30 g EPDM rubber was added to 270 g cyclohexane. After the colloid swelled for 15 hours, it was sheared and dispersed in a high-speed mixer for about half an hour to obtain an EPDM rubber solution. (6) Add 5 g of 30% by mass zinc stearate (5 phr) dispersion in cyclohexane to the EPDM solution of step (5), stir for 10 minutes, then add 5 g of a mixed cyclohexane dispersion of accelerator DM and accelerator TMTD, including 6% accelerator DM (1 phr) and 9% accelerator TMTD (1.5 phr), and stir in a high-speed stirrer at room temperature for 30 minutes, then add 30 g of 30% double-layer modified hollow glass microsphere (30 phr) dispersion in cyclohexane, stir at low speed for 1 hour, and then perform vacuum distillation at 90° C. to remove and recover the cyclohexane solvent, take out the solid wet mixed rubber material and dry it at 90° C. to obtain a mixed rubber; (7) Take out the mixed rubber material after the solvent is removed in step (6), add 0.45g sulfur (1.5phr) on an open mill and thin it twice to make a 2mm thick sheet. After standing for 10 hours, put the sheet into a vulcanizer for vulcanization. The vulcanization temperature is 150℃, the vulcanization pressure is 20MPa, and the vulcanization time is T90+3min.

[0022] Example 2 A method for preparing a hollow glass microsphere / rubber composite material comprises the following steps: (1) Prepare 250 mL of 5% tetramethylammonium hydroxide aqueous solution, add 25 g of hollow glass microspheres with a particle size of 20 μm, stir at 60°C for 1 hour, filter and wash the hollow glass microspheres with deionized water until the pH value of the filtrate is in the range of 8 to 9, and obtain activated hollow glass microspheres; (2) adding deionized water to the hollow glass microspheres activated in step (1) to prepare a dispersion with a mass fraction of 10%, stirring to uniformly disperse the hollow glass microspheres in the water; adding 1 g of hexamethyldisilazane, adding ammonia water to adjust the pH value of the dispersion to 9, heating to 50° C. and keeping the temperature constant for 2 hours; then heating to 70° C. and keeping the temperature constant for 2 hours to obtain a dispersion of hollow glass microspheres modified with a silane coupling agent; (3) adding a 10% sulfuric acid solution to the reaction system of step (2), adjusting the pH value of the dispersion to 8, adding 10 g of a 10% polyvinyl alcohol aqueous solution, stirring at room temperature 25° C. for 1 hour to disperse uniformly, and obtaining a polymer-modified hollow glass microsphere dispersion; (4) spray drying the dispersion obtained in step (3), setting the spray drying inlet temperature to 250° C., the outlet temperature to 100° C., and the feed rate to 40 rpm, to obtain a final double-layer modified hollow glass microsphere product; (5) EPDM rubber (100 phr): 30 g EPDM rubber was added to 270 g cyclohexane. After the colloid swelled for 15 hours, it was sheared and dispersed in a high-speed mixer for about half an hour to obtain an EPDM rubber solution. (6) Add 5 g of 30% by mass zinc stearate (5 phr) in cyclohexane dispersion to the EPDM solution of step (5), stir for 10 minutes, then add 5 g of a mixed cyclohexane dispersion of accelerator DM and accelerator TMTD, including 0.3 g (1 phr) accelerator DM and 0.45 g (1.5 phr) accelerator TMTD, and stir in a high-speed stirrer at room temperature for 30 minutes, then add 24 g of 50% double-layer modified hollow glass microsphere (40 phr) in cyclohexane dispersion, stir for 2 hours, and then perform vacuum distillation at 90° C. to remove the cyclohexane solvent, take out the solid wet mixed rubber material and dry it at 90° C. to obtain a mixed rubber; (7) Take out the mixed rubber material after the solvent is removed in step (6), add 0.45g sulfur (1.5phr) on an open mill and thin it twice to make a 2mm thick sheet. After standing for 10 hours, put the sheet into a vulcanizer for vulcanization. The vulcanization temperature is 150℃, the vulcanization pressure is 20MPa, and the vulcanization time is T90+3min.

[0023] Example 3 A method for preparing a hollow glass microsphere / rubber composite material comprises the following steps: (1) Prepare 250 mL of 10% sodium hydroxide aqueous solution, add 25 g of hollow glass microspheres with a particle size of 40 μm, stir at 60°C for 1 hour, filter and wash the hollow glass microspheres with deionized water until the pH value of the filtrate is in the range of 8 to 9, and obtain activated hollow glass microspheres; (2) adding deionized water to the hollow glass microspheres activated in step (1) to prepare a dispersion with a mass fraction of 10%, starting stirring to uniformly disperse the hollow glass microspheres in the water; adding 0.1 g of vinyltrimethoxysilane and 1 g of ammonia water to adjust the pH value of the dispersion to 9, heating the dispersion to 50° C. and keeping the temperature constant for 2 hours; then heating the dispersion to 70° C. and keeping the temperature constant for 2 hours to obtain a dispersion of hollow glass microspheres modified with a silane coupling agent; (3) adding a 10% sulfuric acid solution to the reaction system of step (2), adjusting the pH value of the dispersion to 6-7, and then adding 5 g of a 10% polyvinyl acetate aqueous solution, stirring at room temperature for 2 hours to disperse uniformly, to obtain a polymer-modified hollow glass microsphere dispersion; (4) spray drying the dispersion obtained in step (3), setting the spray drying inlet temperature to 250° C., the outlet temperature to 100° C., and the feed rate to 35 rpm, to obtain a final double-layer modified hollow glass microsphere product; (5) EPDM rubber (100 phr): 30 g EPDM rubber was added to 270 g cyclohexane. After the colloid swelled for 15 hours, it was sheared and dispersed in a high-speed mixer for about half an hour to obtain an EPDM rubber solution. (6) Add 5 g of 30% by mass zinc stearate (5 phr) in cyclohexane dispersion to the EPDM solution of step (5), stir for 10 minutes, then add 5 g of a mixed cyclohexane dispersion of accelerator DM and accelerator TMTD, including 0.3 g (1 phr) accelerator DM and 0.45 g (1.5 phr) accelerator TMTD, and stir in a high-speed stirrer at room temperature for 30 minutes, then add 30 g of 20% double-layer modified hollow glass microsphere (20 phr) in cyclohexane dispersion, stir for 1 hour, and then perform vacuum distillation at 90° C. to remove the cyclohexane solvent, take out the solid wet mixed rubber material and dry it at 90° C. to obtain a mixed rubber; (7) Take out the mixed rubber material after the solvent is removed in step (6), add 0.45g sulfur (1.5phr) on an open mill and thin it twice to make a 2mm thick sheet. After standing for 10 hours, put the sheet into a vulcanizer for vulcanization. The vulcanization temperature is 150℃, the vulcanization pressure is 20MPa, and the vulcanization time is T90+3min.

[0024] Example 4 Refer to Example 3, except that: in step (5), the EPDM rubber is replaced with natural rubber.

[0025] A method for preparing a hollow glass microsphere / rubber composite material comprises the following steps: (1) Prepare 250 mL of 10% sodium hydroxide aqueous solution, add 25 g of hollow glass microspheres with a particle size of 40 μm, stir at 60°C for 1 hour, filter and wash the hollow glass microspheres with deionized water until the pH value of the filtrate is in the range of 8 to 9, and obtain activated hollow glass microspheres; (2) adding deionized water to the hollow glass microspheres activated in step (1) to prepare a dispersion with a mass fraction of 10%, starting stirring to uniformly disperse the hollow glass microspheres in the water; adding 0.1 g of vinyltrimethoxysilane and 1 g of ammonia water to adjust the pH value of the dispersion to 9, heating the dispersion to 50° C. and keeping the temperature constant for 2 hours; then heating the dispersion to 70° C. and keeping the temperature constant for 2 hours to obtain a dispersion of hollow glass microspheres modified with a silane coupling agent; (3) adding a 10% sulfuric acid solution to the reaction system of step (2), adjusting the pH value of the dispersion to 6-7, and then adding 5 g of a 10% polyvinyl acetate aqueous solution, stirring at room temperature for 2 hours to disperse uniformly, to obtain a polymer-modified hollow glass microsphere dispersion; (4) spray drying the dispersion obtained in step (3), setting the spray drying inlet temperature to 250° C., the outlet temperature to 100° C., and the feed rate to 35 rpm, to obtain a final double-layer modified hollow glass microsphere product; (5) Based on 100 phr of natural rubber dry rubber, dilute the concentrated natural latex with a solid content of 60% to 30%, and take 100 g of the diluted natural latex for later use; (6) Add 5g of a mixed aqueous dispersion of accelerator CZ, accelerator D and zinc oxide to the natural latex of step (5), including 0.3g (1phr) of accelerator CZ, 0.45g (1.5phr) of accelerator TMTD and 1.5g (5phr) of zinc oxide, and stir at room temperature for 30 minutes. Then add 0.45g of stearic acid and 0.45g of microcrystalline wax and stir at 60°C for 1 hour, then add 40g of a 30% aqueous dispersion of double-layer modified hollow glass microspheres and stir at room temperature for 1 hour, and finally add 12g of a 10% aqueous solution of calcium chloride (4phr), stir rapidly at room temperature, and demulsify and flocculate the natural latex; (7) The precipitated rubber block was squeezed and dehydrated, and then dried at 80°C to obtain a mixed rubber. 0.45g of sulfur (1.5phr) was added to the open mill and made into a 2mm thick sheet. After standing for 10 hours, the sheet was placed in a vulcanizer for vulcanization. The vulcanization temperature was 150°C, the vulcanization pressure was 20MPa, and the vulcanization time was T90+3min.

[0026] Comparative Example 1 In this comparative example, hollow glass microspheres are not added as fillers. The specific implementation scheme is as follows: (1) EPDM dry rubber is calculated as 100 phr. 30 g of EPDM rubber is added to 270 g of cyclohexane. After the colloid swells for 15 hours, it is sheared and dispersed in a high-speed mixer for about half an hour to obtain an EPDM rubber solution. (2) Add 5 g of 30% by mass zinc stearate cyclohexane dispersion to the EPDM rubber solution of step (1), stir for 10 minutes, then add 5 g of a mixed cyclohexane dispersion of accelerator DM and accelerator TMTD, which includes 6% accelerator DM and 9% accelerator TMT, and stir in a high-speed mixer at room temperature for 30 minutes, then perform vacuum distillation at 90° C. to remove and recover the cyclohexane solvent, take out the solid wet mixed rubber material, and dry it at 90° C. to obtain a mixed rubber; (3) Take out the mixed rubber material after the solvent is removed in step (6), add 0.45g sulfur (1.5phr) to the open mill and thin it twice to make a 2mm thick sheet. After standing for 10 hours, put the sheet into a vulcanizer at a vulcanizing temperature of 150°C, a vulcanizing pressure of 20MPa, and a vulcanizing time of T90+3min.

[0027] Comparative Example 2 In this comparative example, unmodified hollow glass microspheres are used as fillers. The specific implementation scheme is as follows: (1) EPDM dry rubber is calculated as 100 phr. 30 g of EPDM rubber is added to 270 g of cyclohexane. After the colloid swells for 15 hours, it is sheared and dispersed in a high-speed mixer for about half an hour to obtain an EPDM rubber solution. (2) Add 5 g of 30% by mass zinc stearate cyclohexane dispersion to the EPDM solution of step (1), stir for 10 minutes, then add 5 g of a mixed cyclohexane dispersion of accelerator DM and accelerator TMTD, including 0.3 g of accelerator DM and 0.45 g of accelerator TMTD, and stir in a high-speed stirrer at room temperature for 30 minutes, then add 30 g of 20% unmodified hollow glass microsphere cyclohexane dispersion (particle size 30 μm), stir for 1 hour, and then perform reduced pressure distillation at 90° C. to remove the cyclohexane solvent; (3) Take out the mixed rubber material after the solvent is removed in step (6), add 0.45g sulfur (1.5phr) on the open mill and thin it twice to make a 2mm thick sheet. After standing for 10 hours, put the sheet into a vulcanizer at a vulcanization temperature of 150°C, a vulcanization pressure of 20MPa, and a vulcanization time of T90+3min.

[0028] Performance Evaluation Density: Refer to standard GB / T 533-2008 vulcanized rubber or thermoplastic rubber density test; Tensile properties and elongation at break: refer to the standard GB / T 528-2009 Test of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber. Use a dumbbell-shaped cutter to cut rubber samples. Randomly test 5 samples of each sample and take the average value. The results are shown in the table below.

[0029] By increasing the amount of modified glass microspheres added, the density of the composite rubber is significantly reduced. Compared with EPDM without glass microspheres (Comparative Example 1), as the amount of addition increases (Example 3 < Example 1 < Example 2), the density of the composite rubber continues to decrease, while the tensile strength and elongation at break increase. Compared with the addition of unmodified glass microspheres (Comparative Example 2, 20phr), the mechanical properties of the composite rubber (Example 3) with the same amount of glass microspheres added are also better. The base rubber in Example 4 is natural rubber. After adding glass microspheres, the density of the composite natural rubber is significantly lower than that of pure natural rubber (0.93g / cm 3 ).

[0030] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes that do not deviate from the present invention should be equivalent replacement modes and are included in the protection scope of the present invention.

Claims

1. A method for preparing a hollow glass microsphere / rubber composite material, characterized in that: The following steps are involved: (1) Surface activation of hollow glass microspheres: a certain mass of hollow glass microspheres is added to an alkaline aqueous solution of a certain concentration, stirred and reacted at 25-60°C for 0.5-3h, and then filtered and washed to obtain activated hollow glass microspheres; then the activated hollow glass microspheres are added with water to prepare an aqueous dispersion of a certain concentration; (2) Modifying hollow glass microspheres with silane coupling agent: adding a certain amount of silane coupling agent to the aqueous dispersion prepared in step (1), adjusting the pH to 7.5-10.5, heating to 50-60°C for reaction for 0.5-2h, and then heating to 60-100°C for reaction for 2-4h to graft the silane coupling agent onto the surface of the hollow glass microspheres, thereby obtaining a hollow glass microsphere dispersion modified with a silane coupling agent; (3) Polymer-modified hollow glass microspheres: Weigh a certain amount of polymer, dissolve it in water, add it to the silane coupling agent-modified hollow glass microsphere dispersion obtained in step (2), adjust the pH to 6-9, and react at 20-90° C. for 0.5-2 h to obtain a polymer-modified hollow glass microsphere dispersion; (4) spray drying: spray drying the polymer-modified hollow glass microsphere dispersion of step (3) to obtain surface-modified hollow glass microsphere powder; (5) Wet mixing of hollow glass microsphere / rubber composite: Add the rubber additive dispersion except the vulcanizer and the surface modified hollow glass microsphere powder dispersion into the rubber dispersion or oil-based solution, disperse them evenly, and obtain the mixed rubber after flocculation precipitation or heating to remove the solvent. Then add the vulcanizer on the open mill and vulcanize it to obtain the mixed rubber.

2. The preparation method according to claim 1, characterized in that In step (1), the mass percentage concentration of the alkaline aqueous solution is 0.1 to 20%; the alkali includes but is not limited to one or more of sodium hydroxide, potassium hydroxide, sodium bicarbonate, tetramethylammonium hydroxide, and tetrabutylammonium hydroxide.

3. The preparation method according to claim 1, characterized in that: In step (1), the pH value of the washing liquid is in the range of 7 to 9 during washing, and the mass percentage of the activated hollow glass microspheres in the redispersed aqueous dispersion is in the range of 1 to 20%.

4. The preparation method according to claim 1, characterized in that: In step (2), the silane coupling agent is an alkoxysilane coupling agent, a silazane coupling agent and a silicone oil, including but not limited to bis-[γ-(triethoxysilyl)propyl] tetrasulfide, 3-glycidyloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, dimethyldiethoxysilane, vinyltrimethoxysilane, hexamethyldisilazane, hydroxy silicone oil, hydrogen silicone oil, vinyl silicone oil; the amount of the silane coupling agent used is 0.1% to 20% of the mass of the hollow glass microspheres after activation described in step (1).

5. The preparation method according to claim 1, characterized in that: In step (3), the polymer includes but is not limited to polyethylene glycol, polyvinyl alcohol, polyacrylic acid, polyvinyl pyrrolidone, hydrolyzed maleic anhydride, polyvinyl acetate, ethylene-vinyl acetate copolymer and other hydrophilic polymers, or natural rubber, latex polystyrene butadiene rubber latex, nitrile latex, chloroprene rubber latex, bio-based itaconate rubber and other water-based rubber latex or solution polystyrene butadiene rubber, EPDM rubber, polybutadiene rubber and other oil-based rubber solutions. The amount of polymer used is 1 to 20% of the mass of the hollow glass microspheres after activation described in step (1).

6. The preparation method according to claim 1, characterized in that: In step (4), the inlet temperature of the spray drying is 200-350°C, and the outlet temperature is 80-110°C.

7. The preparation method according to claim 1, characterized in that: In step (5), the rubber additives include one or more of a demulsifier, an accelerator, a vulcanizer, a vulcanization activator, an antioxidant, and a softener; wherein the demulsifier includes one or more of an acid such as formic acid, acetic acid, or a salt such as zinc sulfate, calcium chloride, magnesium chloride, and sodium chloride; the accelerator includes one or more of accelerator CZ, accelerator D, accelerator DM, and accelerator TMTD; the vulcanizer includes one or two of sulfur, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane, and 2,4-dichloroperoxybenzoyl; the vulcanization activator includes stearic acid. One or more of zinc tartrate, stearic acid, and zinc oxide; the softener includes one or more of paraffin, microcrystalline wax, cyclohexane oil, and coumarone resin; among the rubber additives, the demulsifier is used in an amount of 0-20 parts by weight, the accelerator is added in an amount of 0.5-5 parts by weight, the vulcanizer is added in an amount of 0.5-5 parts by weight, the vulcanizing agent is added in an amount of 1-5 parts by weight, the antioxidant is added in an amount of 1-2 parts by weight, and the softener is added in an amount of 1-2 parts; except for the demulsifier, it is dispersed in water or an organic solvent in proportion to prepare a rubber additive dispersion with a mass concentration of 10-40%; the demulsifier is separately prepared into a 1-20% solution.

8. The preparation method according to claim 1, characterized in that: The surface modified hollow glass microsphere powder is used in an amount of 5 to 60 parts by weight and is prepared into a water or organic dispersion with a mass concentration of 15 to 50%.

9. The preparation method according to claim 1, characterized in that: The rubber is selected from natural rubber and / or synthetic rubber, including but not limited to one or more of natural rubber, emulsion-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, nitrile rubber, butadiene rubber, ethylene propylene diene monomer rubber, and bio-based itaconate rubber; the rubber is formulated into an aqueous dispersion or dissolved in an organic solvent to prepare a rubber oil-based solution, and the mass concentration of the rubber is 1 to 60% based on 100 parts by weight of the rubber dry rubber.

10. The preparation method according to claim 1, characterized in that: When one or more water-based rubber latexes such as natural rubber, latex polystyrene butadiene rubber, and bio-based itaconate rubber are used, a water dispersion of rubber additives other than a vulcanizer is poured into the rubber latex, and after shearing and dispersing for 0.5 to 2 hours, a water dispersion of surface-modified hollow glass microbeads is added, and the speed is reduced and stirred and dispersed for 0.5 to 2 hours, and finally a demulsifier solution is added for flocculation and precipitation, and the mixture is filtered, and the solid wet mixed rubber material is taken out and dried to obtain a mixed rubber; When one or more of oil-based rubbers including but not limited to solution-polymerized styrene-butadiene rubber, nitrile rubber, butadiene rubber, ethylene-propylene-diene rubber and the like are used, a dispersion of rubber additives other than a vulcanizing agent is poured into a rubber solution, after shearing and dispersion for 0.5 to 2 hours, an organic dispersion of surface-modified hollow glass microspheres is added, the speed is reduced and stirred and dispersed for 0.5 to 2 hours, then the organic solvent is recovered by vacuum distillation, and a solid wet-mixed rubber material is taken out and dried to obtain a mixed rubber; Finally, a vulcanizing agent is added to the mixed rubber on an open mixer, and then vulcanization is performed to obtain a hollow glass microsphere / rubber composite material.

Citation Information

Cited By

  • Lightweight shockproof sole for air wave shoes and preparation method of lightweight shockproof sole

    CN120157980A

  • High-resilience rubber material and preparation method thereof

    CN120192598A

  • Silica particle coated hollow glass bead and rubber composite material thereof

    CN120665350A