A compatibilizer for bonding metal and plastic and its preparation process
Through the composite and melt extrusion process of difunctional agglomerated polyamide amine with dibutyl maleate and maleic anhydride, high-efficiency metal and plastic compatible agents are prepared, which solves the problem that existing compatible agents are easily sublimated and utilized at high temperatures. The problem of low rate significantly improves the grafting rate and bonding strength, and improves the bonding force between metal and plastic.
Patent Information
- Application Number
- CN202411075098.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing metal and plastic compatible agents are easy to sublimate at high temperatures and have low utilization, resulting in low grafting efficiency and insufficient bonding strength, which affects the mechanical properties and durability of composite materials.
The hydroxyl and siloxane groups in the difunctional agglomerated polyamide are used to combine dibutyl maleate and maleic anhydride to prepare a compatible agent through melt extrusion process, and the hydroxyl groups and siloxane groups in the difunctional agglomerated polyamide are used to improve compatibility. The bonding is enhanced by ultrasonic treatment to form a network structure to enhance adhesion.
It effectively improves the grafting rate and bonding strength, improves the bonding force between metal and plastic, and the preparation process avoids the use of acetone, and improves the water resistance and blending rate of the compatible agent.
Smart Images

Figure CN118599252B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer chemistry, in particular to a compatibilizer for bonding metal and plastic and a preparation process thereof. Background Art
[0002] In modern materials science and engineering technology, composite materials of metal and plastic are widely used in industries such as automobiles, aviation, electronics, construction, packaging, and medical equipment because they combine the strength of metals with the light weight and portability of plastics.
[0003] However, the poor compatibility of metal and plastic interface leads to weak bonding force, which limits the mechanical properties and durability of composite materials. Current compatibilizer technology is mostly focused on single modification, such as maleic anhydride is often selected as polar monomer in industry, and grafted polyolefin is melt-extruded by twin-screw extruder, because the cost of maleic anhydride is low, and the polarity is high, and grafting reaction is easy to occur under the action of high temperature and initiator, which is suitable for industrial large-scale production. However, the disadvantages of low grafting efficiency of compatibilizer caused by the easy sublimation and low utilization rate of maleic anhydride, as well as the problem of a large amount of maleic anhydride remaining in the product, have not been well solved. Thereby causing a large amount of irritating gas to be produced when synthesizing compatibilizer, which can cause a certain amount of damage to the respiratory tract and eyes of human body. Moreover, the bonding strength is low when such compatibilizer is used for metal and plastic.
[0004] Therefore, it has become an urgent need in the industry to develop a compatibilizer and preparation process with high grafting rate and high bonding strength to enhance the bonding strength between metal and plastic. Summary of the invention
[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a compatibilizer for bonding metals and plastics and a preparation process thereof.
[0006] A preparation process of a compatibilizer for bonding metal to plastic, comprising the following steps:
[0007] S1: Preparation of bifunctional polyamidoamine
[0008] Dissolving N,N'-methylenebisacrylamide in an ethanol aqueous solution, adding 3-aminopropyltriethoxysilane and ethanolamine to react, thereby obtaining a bifunctional polyamidoamine;
[0009] S2: Preparation of compatibilizer premix
[0010] Dibutyl maleate, maleic anhydride and an initiator are mixed and added to polypropylene, and then bifunctional polyamide amine is added to obtain a premix;
[0011] S3: Preparation of compatibilizer
[0012] The compatibilizer is obtained by melt extrusion of the premix.
[0013] Optionally, step S1 of preparing the bifunctional polyamidoamine specifically comprises the following steps:
[0014] S1.1: mixing ethanol and water uniformly to obtain an ethanol aqueous solution;
[0015] S1.2: Dissolve 30-32 parts by weight of N,N'-methylenebisacrylamide in an ethanol aqueous solution, stir magnetically at room temperature for 10-15 minutes, then slowly add 35-38 parts by weight of 3-aminopropyltriethoxysilane and 2-3 parts by weight of ethanolamine under magnetic stirring at 30-40°C, and react for 2-3 hours to obtain a bifunctional polyamide amine.
[0016] Optionally, the preparation of the compatibilizer premix in step S2 specifically comprises the following steps:
[0017] S2.1: 3-5 parts by weight of dibutyl maleate, 8-10 parts by weight of maleic anhydride and 0.1-0.2 parts by weight of an initiator are mixed and stirred thoroughly to prepare a mixed liquid;
[0018] S2.2: After the mixed liquid is stirred evenly, it is added into 120-130 parts by weight of polypropylene and stirred for pre-dispersion, then added into a high-speed mixer for mixing, and then 3-5 parts by weight of bifunctional polyamide amine is added and mixed for 3-5 minutes to obtain a premix.
[0019] Optionally, the preparation of the compatibilizer in step S3 specifically comprises the following steps:
[0020] The premix is poured into a twin-screw extruder, melt-extruded through the twin-screw extruder, and then ultrasonic treatment is applied. The feed is adjusted, and the current is maintained within the range of 7-8A, and then melt-grafting extrusion granulation is performed to obtain a compatibilizer.
[0021] Optionally, in step S1.1, ethanol and water are mixed in a weight ratio of 1:1-2.
[0022] Optionally, in step S2.1, the initiator is dicumyl peroxide.
[0023] Optionally, the mixing time in the high-speed mixer in step S2.2 is 3-5 min.
[0024] Optionally, the specific parameters of the twin-screw extruder melt extrusion are a processing temperature of 160-180° C. and a screw speed of 500-550 r / min.
[0025] Optionally, the specific parameter of the ultrasonic treatment is a power of 500-520W.
[0026] A compatibilizer for bonding metal to plastic is prepared by any of the above-mentioned preparation processes for a compatibilizer for bonding metal to plastic.
[0027] Compared with the prior art, the present invention has at least the following beneficial effects:
[0028] 1. The present invention obtains a binary polar monomer by compounding dibutyl maleate and maleic anhydride, and then melt-grafting polypropylene with the composite monomer. Although maleic anhydride has a low melting point and is easy to sublime, its polarity is relatively high. After dibutyl maleate is selected to dissolve and coat maleic anhydride, the concentration of dibutyl maleate is large, the boiling point is relatively high, and the intermolecular force protects maleic anhydride, so the utilization rate of maleic anhydride can be effectively improved. Polypropylene with anhydride groups is more likely to react with dibutyl maleate, thereby effectively improving the grafting rate. At the same time, the preparation process avoids the use of acetone, improves the blending rate of the monomers, and the synthesized compatibilizer has good water resistance.
[0029] 2. The present invention adds a bifunctional polyamide amine. The hydroxyl group in the bifunctional polyamide amine provides hydrophilicity, which helps to wet the metal surface, while the siloxane group provides hydrophobicity, stabilizes the plastic interface, balances the compatibility, and promotes compatibility. The silane group also forms a stable silicon-oxygen bond, such as a Si-O-Si bond, by reacting with the metal surface to provide a strong bond. At the same time, the siloxane group provides flexibility in the plastic to enhance compatibility. The amide group forms a chemical bond with the metal surface and reacts with the plastic chain to form a network structure through physical entanglement, thereby enhancing the interfacial adhesion. The addition of the bifunctional polyamide amine can effectively increase the bonding strength between the metal and the plastic and improve the bonding strength between the metal and the plastic. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.
[0031] Figure 1 This is a process flow chart for preparing a compatibilizer for bonding metals to plastics used in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] The following is a detailed description of a compatibilizer for bonding metal and plastic and its preparation process provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for more specific description of the embodiments, and are not intended to specifically limit the present invention. Example 1
[0033] A process for preparing a compatibilizer for bonding metal to plastic, such as Figure 1 As shown, the following steps are included:
[0034] S1: Preparation of bifunctional polyamidoamine
[0035] S1.1: mixing ethanol and water in a weight ratio of 1:1 to obtain an ethanol aqueous solution;
[0036] S1.2: 30 parts by weight of N,N'-methylenebisacrylamide were dissolved in an ethanol aqueous solution, and magnetically stirred at room temperature for 10 minutes. Then, 35 parts by weight of 3-aminopropyltriethoxysilane and 2 parts by weight of ethanolamine were slowly added under magnetic stirring at 30°C, and the mixture was reacted for 2 hours to obtain a bifunctional polyamidoamine.
[0037] S2: Preparation of compatibilizer premix
[0038] S2.1: 3 parts by weight of dibutyl maleate, 8 parts by weight of maleic anhydride and 0.1 parts by weight of dicumyl peroxide are mixed and stirred thoroughly to prepare a mixed liquid;
[0039] S2.2: After the mixed liquid is stirred evenly, it is added to 120 parts by weight of polypropylene and stirred for pre-dispersion, and then added to a high-speed mixer and mixed for 3 minutes, and then 3 parts by weight of bifunctional polyamide amine are added and mixed for 3 minutes to obtain a premix;
[0040] S3: Preparation of compatibilizer
[0041] The premix is poured into a twin-screw extruder, melt-extruded through the twin-screw extruder, and then subjected to ultrasonic treatment, wherein the specific parameters are processing temperature at 160°C, screw speed at 500r / min, ultrasonic power at 500W, and feed is adjusted to maintain the current within the range of 7A before melt grafting extrusion granulation to obtain a compatibilizer. Example 2
[0042] A process for preparing a compatibilizer for bonding metal to plastic, such as Figure 1 As shown, the following steps are included:
[0043] S1: Preparation of bifunctional polyamidoamine
[0044] S1.1: mixing ethanol and water in a weight ratio of 1:2 to obtain an ethanol aqueous solution;
[0045] S1.2: 32 parts by weight of N, N'-methylenebisacrylamide were dissolved in an ethanol aqueous solution, and magnetically stirred at room temperature for 10 minutes. Then, 38 parts by weight of 3-aminopropyltriethoxysilane and 3 parts by weight of ethanolamine were slowly added under magnetic stirring at 30°C, and the mixture was reacted for 2 hours to obtain a bifunctional polyamidoamine.
[0046] S2: Preparation of compatibilizer premix
[0047] S2.1: 5 parts by weight of dibutyl maleate, 10 parts by weight of maleic anhydride and 0.2 parts by weight of dicumyl peroxide are mixed and stirred thoroughly to prepare a mixed liquid;
[0048] S2.2: After the mixed liquid is stirred evenly, it is added to 130 parts by weight of polypropylene and stirred for pre-dispersion, and then added to a high-speed mixer and mixed for 3 minutes, and then 5 parts by weight of bifunctional polyamide amine are added and mixed for 3 minutes to obtain a premix;
[0049] S3: Preparation of compatibilizer
[0050] The premix is poured into a twin-screw extruder, melt-extruded through the twin-screw extruder, and then subjected to ultrasonic treatment, wherein the specific parameters are processing temperature at 160°C, screw speed at 500r / min, ultrasonic power at 500W, and feed is adjusted to maintain the current within the range of 7A before melt grafting extrusion granulation to obtain a compatibilizer. Example 3
[0051] A process for preparing a compatibilizer for bonding metal to plastic, such as Figure 1 As shown, the following steps are included:
[0052] S1: Preparation of bifunctional polyamidoamine
[0053] S1.1: mixing ethanol and water in a weight ratio of 1:1 to obtain an ethanol aqueous solution;
[0054] S1.2: 30 parts by weight of N,N'-methylenebisacrylamide were dissolved in an ethanol aqueous solution, and magnetically stirred at room temperature for 15 minutes. Then, 35 parts by weight of 3-aminopropyltriethoxysilane and 2 parts by weight of ethanolamine were slowly added under magnetic stirring at 40°C, and reacted for 3 hours to obtain a bifunctional polyamidoamine;
[0055] S2: Preparation of compatibilizer premix
[0056] S2.1: 3 parts by weight of dibutyl maleate, 8 parts by weight of maleic anhydride and 0.1 parts by weight of dicumyl peroxide are mixed and stirred thoroughly to prepare a mixed liquid;
[0057] S2.2: After the mixed liquid is stirred evenly, it is added to 120 parts by weight of polypropylene and stirred for pre-dispersion, and then added to a high-speed mixer and mixed for 5 minutes, and then 3 parts by weight of bifunctional polyamide amine are added and mixed for 5 minutes to obtain a premix;
[0058] S3: Preparation of compatibilizer
[0059] The premix is poured into a twin-screw extruder, melt-extruded through the twin-screw extruder, and then subjected to ultrasonic treatment, wherein the specific parameters are processing temperature at 180°C, screw speed at 550r / min, ultrasonic power at 520W, and the feed is adjusted to maintain the current within the range of 8A before melt grafting extrusion granulation to obtain a compatibilizer.
[0060] Comparative Example 1
[0061] Compared with Example 1, the difference of Comparative Example 1 is that step S2.1 of Comparative Example 1 is replaced by "mixing 3 parts by weight of acetone, 8 parts by weight of maleic anhydride and 0.1 parts by weight of diisopropylbenzene peroxide, and dissolving them in a 50°C water bath to prepare a mixed liquid", and the other steps remain unchanged to prepare the compatibilizer, which is recorded as Comparative Example 1.
[0062] The total grafting rate of the compatibilizers prepared in Examples 1-3 and Comparative Example 1 was measured. The measurement results are shown in Table 1.
[0063] Table 1. Grafting rate measurement results of Examples 1-3 and Comparative Example 1
[0064]
[0065] It can be seen from Table 1 that the data of Comparative Example 1 is significantly lower than that of Example 1, indicating that the grafting rate is effectively improved by compounding dibutyl maleate and maleic anhydride to obtain a binary polar monomer and then using the composite monomer to melt-graft polypropylene.
[0066] Comparative Example 2
[0067] Compared with Example 1, the difference of Comparative Example 2 is that the bifunctional polyamide amine in step S1 and step S2.2 is removed in Comparative Example 2, and the compatibilizer is prepared without changing the other steps, which is recorded as Comparative Example 2.
[0068] The compatibilizers prepared in Examples 1-3 and Comparative Example 2 were used to prepare metal and plastic composite materials, combined with metal parts through a particle nano-injection molding process, and the nano-injection molding bonding strength was tested with a tensile instrument. The nano-injection molding bonding strength test results are shown in Table 2.
[0069] Table 2. Binding strength test results of Examples 1-3 and Comparative Example 2
[0070]
[0071] It can be seen from the data in Table 2 that the nano-injection molding bonding strength of Comparative Example 1 is significantly lower than that of the embodiment, indicating that the addition of bifunctional polyamide amine can effectively increase the bonding strength between metal and plastic and improve the bonding force between metal and plastic.
[0072] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A process for preparing a compatibilizer for bonding metal to plastic, characterized in that: The steps include: S1: Preparation of bifunctional polyamidoamine Dissolving N,N'-methylenebisacrylamide in an ethanol aqueous solution, adding 3-aminopropyltriethoxysilane and ethanolamine to react, thereby obtaining a bifunctional polyamidoamine; S2: Preparation of compatibilizer premix Dibutyl maleate, maleic anhydride and an initiator are mixed and added to polypropylene, and then bifunctional polyamide amine is added to obtain a premix; S3: Preparation of compatibilizer The premix is poured into a twin-screw extruder, melt-extruded through the twin-screw extruder, and then ultrasonic treatment is applied, the feed is adjusted, and the current is maintained within the range of 7-8A, and then melt-grafted extrusion granulation is performed to obtain a compatibilizer; Among them, the specific parameters of the twin-screw extruder melt extrusion are processing temperature at 160-180°C and screw speed at 500-550r / min; The specific parameters of ultrasonic treatment are power of 500-520W.
2. The process for preparing a compatibilizer for bonding metal to plastic according to claim 1, characterized in that: Step S1: Preparation of bifunctional polyamidoamine, specifically comprising the following steps: S1.1: mixing ethanol and water uniformly to obtain an ethanol aqueous solution; S1.2: Dissolve 30-32 parts by weight of N,N'-methylenebisacrylamide in an ethanol aqueous solution, stir magnetically at room temperature for 10-15 minutes, then slowly add 35-38 parts by weight of 3-aminopropyltriethoxysilane and 2-3 parts by weight of ethanolamine under magnetic stirring at 30-40°C, and react for 2-3 hours to obtain a bifunctional polyamide amine.
3. The process for preparing a compatibilizer for bonding metal to plastic according to claim 2, characterized in that: Step S2: Preparation of compatibilizer premix, specifically comprising the following steps: S2.1: 3-5 parts by weight of dibutyl maleate, 8-10 parts by weight of maleic anhydride and 0.1-0.2 parts by weight of an initiator are mixed and stirred thoroughly to prepare a mixed liquid; S2.2: After the mixed liquid is stirred evenly, it is added into 120-130 parts by weight of polypropylene and stirred for pre-dispersion, then added into a high-speed mixer for mixing, and then 3-5 parts by weight of bifunctional polyamide amine is added and mixed for 3-5 minutes to obtain a premix.
4. The process for preparing a compatibilizer for bonding metal to plastic according to claim 2, characterized in that: In step S1.1, ethanol and water are mixed in a weight ratio of 1:1-2.
5. The process for preparing a compatibilizer for bonding metal to plastic according to claim 3, characterized in that: In step S2.1, the initiator is dicumyl peroxide.
6. The process for preparing a compatibilizer for bonding metal to plastic according to claim 3, characterized in that: The mixing time in the high-speed mixer in step S2.2 is 3-5 minutes.
7. A compatibilizer for bonding metal and plastic, characterized in that: The compatibilizer is prepared by the preparation process of a compatibilizer for bonding metal and plastic as described in any one of claims 1 to 6.
Citation Information
Patent Citations
Polyamide-polyolefin copolymer
CN103261282A
Hyperbranched polyamide modified polypropylene composite material and preparation method thereof
CN106995550A