Rubber sealing element for low-temperature refrigeration of marine container

By mixing EPDM rubber with methyl vinyl silicone rubber and adding modified light calcium carbonate and other raw materials, the problem of performance degradation of traditional rubber seals in low-temperature environments has been solved, and the low-temperature resistance and aging resistance have been improved, ensuring the stability and service life of the seals in low-temperature environments.

CN118931054APending Publication Date: 2024-11-12ANHUI YONGZHENG SEAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411279912.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional EPDM rubber seals tend to harden and lose resilience under prolonged low-temperature conditions, leading to a decline in sealing performance. Furthermore, the aging process is accelerated under the combined effects of low temperature, moisture, and oxygen, which affects the sealing effect and service life.

Method used

Rubber seals are prepared by mixing EPDM rubber and methyl vinyl silicone rubber, adding carbon black and modified light calcium carbonate, and then mixing and vulcanizing. The modified light calcium carbonate is treated with silane coupling agent KH-560 and p-aminodiphenylamine to improve its dispersibility and anti-aging properties.

Benefits of technology

It improves the low-temperature resistance, mechanical properties, and aging resistance of rubber seals, ensuring stable sealing performance in low-temperature environments and extending service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931054A_ABST
    Figure CN118931054A_ABST
Patent Text Reader

Abstract

The invention discloses a rubber sealing piece for low-temperature refrigeration of a marine container, and belongs to the technical field of rubber materials, the rubber sealing piece comprises a U-shaped clamping groove fixing end and an O-shaped nitrogen isolation end, and the U-shaped clamping groove fixing end comprises a sawtooth structure; the U-shaped clamping groove fixing end and the O-shaped nitrogen isolation end are both prepared from, by weight, 60-85 parts of ethylene propylene diene monomer, 20-30 parts of methyl vinyl silicone rubber, 20-30 parts of carbon black, 8-12 parts of modified light calcium carbonate, 3-6 parts of zinc oxide, 0.5-1 part of accelerant, 0.5-1 part of vulcanizing agent and 5-15 parts of rubber oil. The rubber sealing element for low-temperature refrigeration of the marine container has excellent low-temperature resistance, mechanical property and aging resistance, can be in a low-temperature environment for a long time, is not easy to crack, harden and the like, meets the use requirements in long-term large-temperature-difference and low-temperature environments, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber materials, and in particular relates to a rubber seal for low-temperature refrigeration of shipping containers. Background Art

[0002] Rubber seals used for low-temperature refrigeration in shipping containers need to have good low-temperature resistance and sealing effect. Ethylene propylene diene monomer (EPDM) is widely used in the preparation of shipping container seals due to its good elasticity and excellent heat resistance, low-temperature resistance, oil resistance, weather resistance and electrical insulation.

[0003] Although traditional EPDM seals have certain low-temperature resistance, due to the generally long distance of sea transportation, the weather resistance and heat insulation of traditional EPDM rubber seals are difficult to play their advantages in long-term sea transportation. At the same time, some materials need to be refrigerated inside the container for a long time. When in a low-temperature environment for a long time, conventional EPDM sealing rubber materials will harden, weaken their resilience, become brittle, and other problems, resulting in reduced sealing performance. It is difficult to meet the requirements of long-term use in large temperature differences and low-temperature environments, which in turn affects the sealing effect of seals in low-temperature refrigerated containers, and may cause problems such as poor sealing, air leakage or water seepage. Although the low-temperature environment slows down the speed of certain chemical reactions, under certain specific conditions (such as the combined effect of low temperature, moisture, oxygen, etc.), the aging process of rubber seals may be accelerated. The aged seals will crack, harden or soften, which seriously affects their sealing effect and service life. Summary of the invention

[0004] The present invention aims to provide a low-temperature refrigeration rubber seal for shipping containers, in order to improve the low-temperature resistance of the rubber seal which is insufficient under low-temperature conditions for a long time, thereby causing cracking, hardening and other problems.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A low-temperature refrigeration rubber seal for a shipping container, comprising a U-shaped slot fixing end and an O-shaped nitrogen isolation end, wherein the U-shaped slot fixing end comprises a serrated structure, and the U-shaped slot fixing end and the O-shaped nitrogen isolation end are both prepared from the following raw materials in parts by weight:

[0007] 60-85 parts of EPDM rubber, 20-30 parts of methyl vinyl silicone rubber, 20-30 parts of carbon black, 8-12 parts of modified light calcium carbonate, 3-6 parts of zinc oxide, 0.5-1 parts of accelerator, 0.5-1 parts of vulcanizer, and 5-15 parts of rubber oil.

[0008] As a further solution of the present invention, the modified light calcium carbonate is prepared by the following steps:

[0009] S1. In a nitrogen atmosphere, silane coupling agent KH-560 and p-aminodiphenylamine are mixed, heated and stirred to react, and cooled to obtain a premixed solution;

[0010] S2, adding light calcium carbonate to the premix and anhydrous ethanol, stirring the reaction, centrifugation filtering, drying, washing, and further drying to obtain modified light calcium carbonate. In the above technical scheme, the epoxy group in the silane coupling agent KH-560 and the amino group of p-aminodiphenylamine are first subjected to a ring-opening reaction to form a p-phenylenediamine anti-aging group, and then the silane coupling agent KH-560 is dehydrated under high temperature conditions so that the coupling agent is firmly grafted on the surface of the light calcium carbonate. On the one hand, the hydroxyl group on the surface of the calcium carbonate is reduced and the surface is grafted with p-aniline macromolecules, which improves the dispersibility and compatibility of calcium carbonate; on the other hand, compared with the direct addition of antioxidants, the antioxidant groups are grafted on the surface of calcium carbonate at this time, which has the advantages of resistance to migration and precipitation and is not easy to fall off, so that the anti-aging effect can be maintained for a longer time, further improving the aging resistance of rubber seals.

[0011] As a further embodiment of the present invention, the usage ratio of silane coupling agent KH-560 and p-aminodiphenylamine in S1 is 1.0-1.1 mL: 0.90-0.95 g.

[0012] As a further embodiment of the present invention, the dosage ratio of light calcium carbonate, premixed liquid and anhydrous ethanol in S2 is 1.5-2.0 g: 4-5 mL: 10 mL.

[0013] As a further embodiment of the present invention, the accelerator is at least one of diphenylguanidine, tetraethylthiuram disulfide, and tetramethylthiuram disulfide.

[0014] As a further embodiment of the present invention, the particle size of the carbon black is 20-40 nm.

[0015] As a further embodiment of the present invention, the carbon black is at least one of white carbon black and black carbon black.

[0016] As a further embodiment of the present invention, the vulcanizing agent is sulfur.

[0017] As a further embodiment of the present invention, the rubber oil is paraffin oil.

[0018] As a further solution of the present invention, the rubber seal raw material is prepared by the following steps:

[0019] Step 1, putting EPDM rubber and methyl vinyl silicone rubber into an internal mixer for internal mixing, then adding carbon black, modified light calcium carbonate, zinc oxide, accelerator, vulcanizing agent and rubber oil, continuing to internal mix, discharging after mixing evenly, and cooling to obtain a mixed rubber;

[0020] Step 2, putting the mixed rubber into an open mixer, mixing, discharging, and cooling to obtain a film;

[0021] Step 3: vulcanize the film and cool it.

[0022] Beneficial effects of the present invention:

[0023] The present invention adopts EPDM rubber and methyl vinyl silicone rubber, and simultaneously adds carbon black, modified light calcium carbonate, zinc oxide, accelerator, vulcanizer and rubber oil, and obtains the raw material of rubber seal through mixing and vulcanization. The present invention mixes EPDM rubber with methyl vinyl silicone rubber. Since the bond energy of the main chain Si-O bond of methyl vinyl silicone rubber is higher than the bond energy of the main chain CC bond of general rubber molecules, it has very excellent high and low temperature resistance, elasticity and good electrical insulation. After blending, the glass transition temperature of EPDM rubber can be reduced, thereby improving the low temperature resistance of EPDM rubber, and then preparing a rubber seal. The obtained rubber seal has good low temperature resistance, mechanical properties and aging resistance.

[0024] In the present invention, carbon black and modified light calcium carbonate are used as reinforcing fillers. Carbon black can form carbon black gel with rubber mix, thereby improving the physical and mechanical properties of the rubber mix, improving the ability to resist permanent compression deformation, and the permanent compression deformation is small. In addition, the morphology of carbon black particles is good in compatibility with rubber, has an obvious reinforcing effect on the rubber mix, improves the tensile stress of the rubber mix, and can also reduce the permanent compression deformation. Although the reinforcing effect of light calcium carbonate is poorer than that of carbon black, it has an improving effect on the tear strength, flexure, resilience and permanent deformation of the rubber mix. Therefore, under the synergistic effect of carbon black and modified light calcium carbonate, the resistance to permanent compression deformation, mechanical properties and aging resistance of the rubber seal are further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described below in conjunction with the accompanying drawings.

[0026] Figure 1 The present invention is a structural schematic diagram of a low-temperature refrigeration rubber seal for a shipping container. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] This embodiment provides a modified light calcium carbonate, and the preparation steps are as follows:

[0030] S1. Under nitrogen atmosphere, 1.0 mL of silane coupling agent KH-560 and 0.90 g of p-aminodiphenylamine were mixed, heated to 115 °C and stirred for 6.5 h, and cooled to obtain a premixed solution;

[0031] S2. Add 1.55 g of light calcium carbonate to 4 mL of premix and 10 mL of anhydrous ethanol, stir and react for 6 h, centrifuge and filter, place in a vacuum drying oven at 120 ° C. and dry for 12 h, take out and wash with anhydrous ethanol for 3 times, continue to place in a vacuum drying oven at 120 ° C. and dry for 3 h to obtain modified light calcium carbonate.

[0032] Example 2

[0033] This embodiment provides a modified light calcium carbonate, and the preparation steps are as follows:

[0034] S1. Under nitrogen atmosphere, 1.0 mL of silane coupling agent KH-560 and 0.90 g of p-aminodiphenylamine were mixed, heated to 115 °C and stirred for 6.5 h, and cooled to obtain a premixed solution;

[0035] S2. Add 1.95 g of light calcium carbonate to 4 mL of premix and 10 mL of anhydrous ethanol, stir and react for 6 h, centrifuge and filter, place in a vacuum drying oven at 120 ° C. and dry for 12 h, take out and wash with anhydrous ethanol for 3 times, continue to place in a vacuum drying oven at 120 ° C. and dry for 3 h to obtain modified light calcium carbonate.

[0036] Example 3

[0037] This embodiment provides a modified light calcium carbonate, and the preparation steps are as follows:

[0038] S1. Under nitrogen atmosphere, 1.1 mL of silane coupling agent KH-560 and 0.94 g of p-aminodiphenylamine were mixed, heated to 120 °C and stirred for 6 h, and cooled to obtain a premixed solution;

[0039] S2. Add 1.8 g of light calcium carbonate to 4.6 mL of premix and 10 mL of anhydrous ethanol, stir and react for 8 h, centrifuge and filter, place in a vacuum drying oven at 120 ° C. and dry for 12 h, take out and wash with anhydrous ethanol 5 times, continue to place in a vacuum drying oven at 120 ° C. and dry for 3 h to obtain modified light calcium carbonate.

[0040] Comparative Example 1

[0041] This comparative example provides a modified light calcium carbonate, and the preparation steps are as follows:

[0042] S1. Add 1.55 g of light calcium carbonate to 10 mL of anhydrous ethanol, stir and react for 6 h, centrifuge and filter, place in a vacuum drying oven at 120 ° C. and dry for 12 h, take out and wash with anhydrous ethanol for 3 times, continue to place in a vacuum drying oven at 120 ° C. and dry for 3 h to obtain modified light calcium carbonate.

[0043] Example 4

[0044] This embodiment provides a low-temperature refrigeration rubber seal for shipping containers, including a U-shaped slot fixing end and an O-shaped nitrogen isolation end, wherein the U-shaped slot fixing end includes a sawtooth structure (the specific structure is shown in FIG. Figure 1 As shown), the U-shaped slot fixing end and the O-shaped nitrogen isolation end are both prepared from the following raw materials in parts by weight:

[0045] 65 parts of EPDM rubber, 20 parts of methyl vinyl silicone rubber, 20 parts of white carbon black (particle size is 20 nm), 8 parts of modified light calcium carbonate in Example 1, 4 parts of zinc oxide, 0.5 parts of diphenylguanidine, 0.5 parts of sulfur, and 8 parts of paraffin oil.

[0046] The steps for preparing the sealing material are as follows:

[0047] Step 1, putting EPDM rubber and methyl vinyl silicone rubber into an internal mixer for internal mixing, then adding white carbon black, modified light calcium carbonate in Example 1, zinc oxide, diphenyl guanidine, sulfur and paraffin oil, continuing to internal mix, discharging after mixing evenly, and cooling to obtain a mixed rubber;

[0048] Step 2, putting the mixed rubber into an open mixer, mixing, discharging, and cooling to obtain a film;

[0049] Step 3: vulcanize the film and cool it.

[0050] Example 5

[0051] The only difference from Example 4 is that:

[0052] The modified light calcium carbonate in Example 1 is replaced by the modified light calcium carbonate in Example 2, and the amount used remains unchanged.

[0053] Example 6

[0054] The only difference from Example 4 is that:

[0055] The modified light calcium carbonate in Example 1 is replaced by the modified light calcium carbonate in Example 3, and the amount used remains unchanged.

[0056] Example 7

[0057] The only difference from Example 4 is that:

[0058] Replace 8 parts of the modified light calcium carbonate in Example 1 with 10 parts of the modified light calcium carbonate in Example 1.

[0059] Example 8

[0060] The only difference from Example 4 is that:

[0061] Replace 8 parts of the modified light calcium carbonate in Example 1 with 12 parts of the modified light calcium carbonate in Example 1.

[0062] Example 9

[0063] The only difference from Example 4 is that:

[0064] The U-shaped slot fixing end and the O-shaped nitrogen isolation end are both prepared from the following raw materials in parts by weight:

[0065] 75 parts of EPDM rubber, 25 parts of methyl vinyl silicone rubber, 25 parts of black carbon black (particle size is 30nm), 9 parts of modified light calcium carbonate in Example 1, 5 parts of zinc oxide, 0.8 parts of tetraethylthiuram disulfide, 0.6 parts of sulfur, and 10 parts of paraffin oil.

[0066] Example 10

[0067] The only difference from Example 4 is that:

[0068] The U-shaped slot fixing end and the O-shaped nitrogen isolation end are both prepared from the following raw materials in parts by weight:

[0069] 85 parts of EPDM rubber, 30 parts of methyl vinyl silicone rubber, 30 parts of carbon black, 11 parts of modified light calcium carbonate in Example 1, 6 parts of zinc oxide, 0.9 parts of tetramethylthiuram disulfide, 0.1 parts of sulfur, and 14 parts of paraffin oil.

[0070] Comparative Example 2

[0071] The only difference from Example 4 is that:

[0072] The modified light calcium carbonate in Example 1 was replaced by the modified light calcium carbonate in Comparative Example 1, and the amount used remained unchanged.

[0073] Comparative Example 3

[0074] The only difference from Example 4 is that:

[0075] Replace 8 parts of the modified light calcium carbonate in Example 1 with 5 parts of the modified light calcium carbonate in Example 1.

[0076] Comparative Example 4

[0077] The only difference from Example 4 is that:

[0078] Replace 8 parts of the modified light calcium carbonate in Example 1 with 15 parts of the modified light calcium carbonate in Example 1.

[0079] Comparative Example 5

[0080] The only difference from Example 4 is that:

[0081] The U-shaped slot fixing end and the O-shaped nitrogen isolation end are both prepared from the following raw materials in parts by weight:

[0082] 65 parts of EPDM rubber, 20 parts of white carbon black (particle size is 20 nm), 8 parts of modified light calcium carbonate in Example 1, 4 parts of zinc oxide, 0.5 parts of diphenylguanidine, 0.5 parts of sulfur, and 8 parts of paraffin oil.

[0083] Comparative Example 6

[0084] The only difference from Example 4 is that:

[0085] The U-shaped slot fixing end and the O-shaped nitrogen isolation end are both prepared from the following raw materials in parts by weight:

[0086] 55 parts of EPDM rubber, 10 parts of methyl vinyl silicone rubber, 35 parts of carbon black, 8 parts of modified light calcium carbonate in Example 1, 6 parts of zinc oxide, 0.9 parts of tetramethylthiuram disulfide, 0.1 parts of sulfur, and 14 parts of paraffin oil.

[0087] The following performance tests were performed on the rubber seals obtained in Example 4, Example 10 and Comparative Examples 2 to 6:

[0088] 1. Tensile strength and elongation at break test: The tensile strength and elongation at break are tested according to DIN 53504-2009 standard.

[0089] 2. Low temperature compression permanent deformation test: The low temperature compression permanent deformation rate is tested using the test standard PV33632010. The low temperature compression permanent deformation test sets the temperature at -40±2℃, the aging time is 24h, and the reading is taken 5s after unloading.

[0090] 3. Low temperature compression load change rate: The low temperature compression load change rate is tested using the PV33642010 test standard. The low temperature compression load change rate sets the temperature to normal temperature (23±2)℃ and low temperature (-40±2)℃ for dynamic compression testing, and is calculated by the following calculation method: (low temperature value - normal temperature value) / normal temperature value. The calculated percentage change rate represents the actual low temperature resistant sealing performance. The lower the value, the better the actual low temperature performance. The above test results are shown in Table 1:

[0091] Table 1

[0092]

[0093]

[0094] 4. Aging resistance test: According to GB / T 3512-2014 "Hot air accelerated aging and heat resistance test for vulcanized rubber or thermoplastic rubber", the aging test was carried out, and the tensile strength and elongation at break of each sample after aging were tested according to the above-mentioned tensile strength and elongation at break test methods, and the retention rate of tensile strength and elongation at break were calculated. In the aging resistance test, the cabinet hot air aging box in method A was used, with 5 ventilation times per hour, a temperature of 200°C, and a time of 72 hours; during the test, each group included 6 samples, and the average value of the test results of each group of 6 samples was taken as the final test result. The above test results are shown in Table 2:

[0095] Table 2

[0096]

[0097]

[0098] It can be seen from Table 1-2 that the tensile strength, elongation at break, low temperature resistance and aging resistance of the rubber seals obtained in Examples 4-10 are better than those obtained in Comparative Examples 2-6. It can be seen that the rubber seals for low temperature refrigeration of shipping containers provided in the present invention have excellent low temperature resistance, aging resistance and mechanical properties, and have good aging resistance and weather resistance when kept at low temperature for a long time, and the mechanical properties of the material are stable, the service life is long, and it has good application prospects.

[0099] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0100] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A low-temperature refrigeration rubber seal for a shipping container, comprising a U-shaped slot fixing end and an O-shaped nitrogen isolation end, wherein the U-shaped slot fixing end comprises a sawtooth structure, characterized in that: The U-shaped slot fixing end and the O-shaped nitrogen isolation end are both prepared from the following raw materials in parts by weight: 60-85 parts of EPDM rubber, 20-30 parts of methyl vinyl silicone rubber, 20-30 parts of carbon black, 8-12 parts of modified light calcium carbonate, 3-6 parts of zinc oxide, 0.5-1 parts of accelerator, 0.5-1 parts of vulcanizer, and 5-15 parts of rubber oil.

2. The rubber seal for low temperature refrigeration of shipping containers according to claim 1, characterized in that: The modified light calcium carbonate is prepared by the following steps: S1. In a nitrogen atmosphere, silane coupling agent KH-560 and p-aminodiphenylamine are mixed, heated and stirred to react, and cooled to obtain a premixed solution; S2. Add light calcium carbonate to the premixed liquid and anhydrous ethanol, stir to react, centrifuge, filter, dry, wash, and continue drying to obtain modified light calcium carbonate.

3. The rubber seal for low temperature refrigeration of a shipping container according to claim 2, characterized in that: The dosage ratio of silane coupling agent KH-560 and p-aminodiphenylamine in S1 is 1.0-1.1 mL: 0.90-0.95 g.

4. The rubber seal for low temperature refrigeration of a shipping container according to claim 2, characterized in that: The dosage ratio of light calcium carbonate, premixed liquid and anhydrous ethanol in S2 is 1.5-2.0 g: 4-5 mL: 10 mL.

5. The rubber seal for low temperature refrigeration of shipping containers according to claim 1, characterized in that: The accelerator is at least one of diphenylguanidine, tetraethylthiuram disulfide and tetramethylthiuram disulfide.

6. The rubber seal for low temperature refrigeration of shipping containers according to claim 1, characterized in that: The particle size of the carbon black is 20-40 nm.

7. The rubber seal for low temperature refrigeration of shipping containers according to claim 1, characterized in that: The carbon black is at least one of white carbon black and black carbon black.

8. The rubber seal for low temperature refrigeration of a shipping container according to claim 1, characterized in that: The vulcanizing agent is sulfur.

9. The rubber seal for low temperature refrigeration of a shipping container according to claim 1, characterized in that: The rubber oil is paraffin oil.

10. The rubber seal for low temperature refrigeration of a shipping container according to claim 1, characterized in that: The rubber seal raw material is prepared by the following steps: Step 1, putting EPDM rubber and methyl vinyl silicone rubber into an internal mixer for internal mixing, then adding carbon black, modified light calcium carbonate, zinc oxide, accelerator, vulcanizing agent and rubber oil, continuing to internal mix, discharging after mixing evenly, and cooling to obtain a mixed rubber; Step 2, putting the mixed rubber into an open mixer, mixing, discharging, and cooling to obtain a film; Step 3: vulcanize the film and cool it.