Tight-fitting trenchless repair material and preparation method thereof

The combination of the new core-shell modifier prepared by emulsion polymerization and SG-3 and SG-5 polyvinyl chloride resins solves the problem of insufficient ring stiffness in existing materials in large-size variable diameter construction, and achieves high ring stiffness and high expansion rate PVC lined tubes, suitable for pipe repairs of multiple diameters.

CN118931069APending Publication Date: 2024-11-12HUNAN DALU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411271375.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing tightly fit non-excavation repair materials cannot guarantee the expansion ring stiffness during large-diameter construction, resulting in insufficient ring stiffness after construction and cannot meet the needs of pipeline repairs of multiple diameters.

Method used

A new core-shell modifier prepared by emulsion polymerization combines SG-3 and SG-5 polyvinyl chloride resins, nano calcium carbonate, calcium zinc stabilizer, lubricant and plasticizer, and through specific mixing and The extrusion process produces high ring stiffness and high expansion rate PVC lined tubes to ensure that the material can maintain high ring stiffness after expansion.

Benefits of technology

The material has been expanded to ≥8KN/m2, which can adapt to pipeline repairs of multiple diameters, enhances the toughness and rigidity of the material, and is suitable for non-excavation and variable diameter repairs in large-sized variable diameter scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005038814740000081
    Figure BDA0005038814740000081
  • Figure BDA0005038814740000082
    Figure BDA0005038814740000082
  • Figure BDA0005038814740000083
    Figure BDA0005038814740000083
Patent Text Reader

Abstract

According to the tightly-attached trenchless repair material and the preparation method thereof, the tightly-attached trenchless repair material adopts a novel core-shell modifier as a toughening agent, when the material is impacted, rubber particles of a core layer generate elastic deformation, the toughness of the material can be obviously improved, the compatibility of a copolymer of a shell layer and a PVC matrix is good, and the toughness of the material can be obviously improved. The butadiene-acrylonitrile polymer can be uniformly dispersed in a PVC matrix to form a three-dimensional network cross-linked structure, and due to the rigidity effect of the butadiene-acrylonitrile polymer, the material is endowed with good rigidity. The material has better thermal expansion ductility, can realize 150% or more expansion construction, so that a single-caliber lining pipe can adapt to original pipelines with more calibers (a DN280 lining pipe can be tightly attached to repair a DN450-caliber damaged pipeline), and can still maintain higher ring stiffness (greater than or equal to 8KN / m < 2 >) after expansion construction; and a better application effect is achieved under the condition that the diameter of the to-be-repaired pipeline is changed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of trenchless repair engineering, and in particular to a tightly fitting trenchless repair material and a preparation method thereof. Background Art

[0002] The principle of the close-fitting trenchless repair method is to use a thermoplastic molding process to repair the inner lining of the pipeline. The main construction process can be summarized as placing the continuous inner lining pipe with a reduced cross-section into the original pipeline, and restoring the cross-section after placement so that its surface fits tightly with the inner wall of the original pipeline. The inner lining pipe is usually made of PVC-U material that can be processed twice. The pipe is folded and formed in the factory, and is heated at the construction site to soften the inner lining pipe. It is pulled into the original pipeline through a traction device, and steam heating and pressurization are used to make it fit tightly with the original pipeline. After cooling, a "pipe in pipe" lining structure is finally formed.

[0003] The tight-fitting PVC lined pipes for trenchless repair currently used in the market are mainly modified with elastomers such as CPE, ACR, polyurethane, and polyolefins to give them shape memory functions. Before use, their cross-sections can be reduced for winding and reeling, and after being introduced into the pipeline, they can be heated to restore their shape and adhere closely to the pipe wall to achieve pipeline repair.

[0004] Chinese patent application CN109810430A discloses a pipe material for pipe repair using thermoplastic molding method using polyvinyl chloride. It mainly solves the problem of softening of PVC liner pipes by heating by using PVC materials modified by polyolefin elastomers such as POE and SEBS, and develops a PVC hard pipe formula with a low glass transition temperature. Although the introduction of elastomers such as POE enhances the toughness of the pipe material, it cannot guarantee the rigidity of the liner pipe after expansion. In the case of a large diameter change construction scenario, the ring stiffness of the material cannot be guaranteed after expansion construction, and the ring stiffness after construction is only 1.5KN / m 2 , it is not suitable for diameter change repair. Summary of the invention

[0005] The present invention provides a tightly fitting trenchless repair material and a preparation method thereof, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0006] In order to achieve the above-mentioned purpose, the embodiment of the present invention provides a close-fitting trenchless repair material and a preparation method thereof, which has a shape memory function, can be folded and wound before use, can be heated to restore the round shape after being introduced into the pipeline, and can be close to the pipe wall to achieve pipeline repair requirements, and has a high ring stiffness (≥10KN / m 2) and a close-fitting PVC liner with high expansion rate and good elongation performance (elongation ≥150%). The liner has better thermal expansion and ductility, and can achieve expansion construction of 150% and above, so that a single-caliber liner can adapt to more calibers of original pipelines, and can still maintain a high ring stiffness (≥8KN / m after expansion and diameter reduction construction) 2 ), which can realize trenchless variable diameter repair in scenarios where the pipeline changes significantly in diameter, and has better application effect when the pipeline to be repaired changes in diameter.

[0007] An embodiment of the present invention provides a tightly fitting trenchless repair material, which includes the following components by weight: 100 parts of polyvinyl chloride resin, 5 to 10 parts of nano calcium carbonate, 5 to 10 parts of a new core-shell modifier, 2 to 4 parts of a calcium zinc stabilizer, 0.2 to 0.4 parts of a lubricant and 3 to 10 parts of a plasticizer.

[0008] According to one aspect of an embodiment of the present invention, the novel core-shell modifier is prepared by emulsion polymerization, with styrene-butadiene rubber as the core and butadiene-acrylonitrile copolymer as the shell.

[0009] According to one aspect of the embodiment of the present invention, the polyvinyl chloride resin is composed of SG-3 type resin and SG-5 type resin in a weight ratio of 1: 1. The SG-3 resin and SG-5 resin are compounded in proportion to ensure material strength and take into account processing performance, which is more suitable for the production of high-performance pipes.

[0010] According to one aspect of an embodiment of the present invention, the lubricant is at least one of PE wax, calcium stearate, and oxidized polyethylene wax.

[0011] According to one aspect of an embodiment of the present invention, the plasticizer is dioctyl terephthalate or epoxidized soybean oil. Based on 100 parts by weight of the polyvinyl chloride resin, the amount of the plasticizer is 3 to 10 parts, preferably 3 to 5 parts. If the amount of the plasticizer is too low, it is difficult to play a plasticizing role. On the contrary, if the content of the plasticizer is higher than 10 parts, the strength of the material is insufficient.

[0012] Based on a general concept of the invention, an embodiment of the present invention provides a method for preparing a tightly fitting trenchless repair material, comprising the following steps:

[0013] S1: According to the formula, polyvinyl chloride resin, nano calcium carbonate, calcium zinc stabilizer and lubricant are weighed and added into a high-speed mixer for mixing, the temperature is raised, and a plasticizer is added for mixing; a new core-shell modifier is added for mixing, and the hot mixed material is transferred into a cold mixing device for mixing and cooling, and then discharged and sieved to obtain a mixed material;

[0014] S2: The mixture is placed at room temperature for aging, and then input into a twin-screw extruder for plasticization and extrusion. After vacuum shaping, folding, pulling, heating, winding and cutting, a tightly fitting non-excavation repair material is obtained. Note: The new core-shell modifier must be added after the liquid plasticizer has been completely absorbed by the polyvinyl chloride resin. The plasticizer, polyvinyl chloride resin and the new core-shell modifier cannot be mixed at the same time. Because when added at the same time, the new core-shell modifier will preferentially absorb the plasticizer, resulting in an uneven mixture.

[0015] According to one aspect of an embodiment of the present invention, in step S1, a plasticizer is added when the temperature rises to 70-80°C; a novel core-shell modifier is added when the temperature rises to 110°C; and when the temperature is 130-135°C, the hot mixture is transferred to a cold mixing device for mixing and cooling until it is discharged below 50°C.

[0016] According to one aspect of the embodiment of the present invention, in step S2, the aging time is 12 to 24 hours.

[0017] According to one aspect of an embodiment of the present invention, the preparation method of the novel core-shell modifier comprises the following steps:

[0018] Deionized water, emulsifier and styrene-butadiene latex are stirred to obtain a core layer pre-emulsion;

[0019] Dissolving the initiator in deionized water to obtain an initiator aqueous solution;

[0020] Add deionized water and 1 / 3 of the core layer pre-emulsion into a four-necked flask, stir and heat, then add an emulsifier and 1 / 3 of the initiator aqueous solution, and react at a constant temperature; slowly dropwise add the remaining core layer pre-emulsion and 1 / 3 of the initiator aqueous solution, heat and react at a constant temperature; dropwise add butadiene, acrylonitrile and the remaining initiator aqueous solution, react, cool to room temperature, adjust the pH value with ammonia water, and obtain a mixed solution;

[0021] A manganese sulfate aqueous solution is added to the mixed solution, and the mixture is demulsified, filtered, washed, and dried to obtain the product.

[0022] According to one aspect of the embodiments of the present invention, the emulsifier is sodium dodecyl sulfate (SDS); and the initiator is potassium polysulfate (KPS).

[0023] The above scheme of the present invention has the following beneficial effects:

[0024] (1) The close-fitting trenchless repair material of the present invention adopts a new core-shell modifier prepared by emulsion polymerization with styrene-butadiene rubber as the core and butadiene-acrylonitrile copolymer as the shell as a toughening agent. When the material is impacted, the rubber particles in the core layer produce elastic deformation, which can significantly improve the toughness of the material. The copolymer in the shell layer has good compatibility with the PVC matrix, so that it can be evenly dispersed in the PVC matrix to form a three-dimensional network cross-linked structure. In addition, due to the rigidity of the butadiene-acrylonitrile polymer itself, the material is endowed with good rigidity. Different from the currently used CPE, ACR, polyurethane, polyolefin and other elastomers as toughening materials for PVC, these low modulus elastomers will sacrifice a certain modulus and rigidity of the material while achieving toughening. The self-made new core-shell modifier is introduced into PVC by blending and melt extrusion. The self-made new core-shell modifier has good compatibility with the PVC matrix. The modified PVC liner pipe not only has good toughness, but also the rigidity of the material can be well guaranteed, so that it can better meet the application requirements. The liner pipe has better thermal expansion and ductility, and can achieve 150% or more expansion construction, so that a single-caliber liner pipe can adapt to more calibers of original pipes (for example: DN280 liner pipe can fit tightly to repair DN450 caliber damaged pipes), and can still maintain a high ring stiffness after expansion construction (≥8KN / m 2 ), which has better application effect when the pipe to be repaired changes its diameter.

[0025] (2) The overall process of the preparation method of the present invention is mature, simple and easy to operate, the equipment can operate continuously, and it can meet the needs of mass production and manufacturing, and has good application prospects. DETAILED DESCRIPTION

[0026] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, they are described in detail below in conjunction with specific embodiments.

[0027] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0028] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0029] Although the introduction of existing elastomers such as POE enhances the toughness of the pipe, it cannot guarantee the rigidity of the liner after expansion. In the case of a large diameter change construction scenario, the ring stiffness of the material after expansion construction cannot be guaranteed. The ring stiffness after construction is only 1.5KN / m. 2 , it is not suitable for diameter change repair and other problems.

[0030] An embodiment of the present invention provides a tightly fitting trenchless repair material, comprising the following components in parts by weight: 100 parts of polyvinyl chloride resin, 5 to 10 parts of nano calcium carbonate, 5 to 10 parts of a new core-shell modifier, 2 to 4 parts of a calcium zinc stabilizer, 0.2 to 0.4 parts of a lubricant and 3 to 10 parts of a plasticizer.

[0031] Based on a general concept of the invention, an embodiment of the present invention provides a method for preparing a tightly fitting trenchless repair material, comprising the following steps:

[0032] S1: According to the components of the formula, polyvinyl chloride resin, nano calcium carbonate, calcium zinc stabilizer and lubricant are weighed and added into a high-speed mixer for mixing. When the temperature rises to 70-80°C, a liquid plasticizer is added, and the mixing is continued until the temperature reaches 110°C. The new core-shell modifier is added, and the mixing is continued until the temperature reaches 130-135°C. The hot mixed material is transferred to a cold mixing device for mixing and cooling until the temperature is below 50°C, and then discharged and sieved to obtain a mixed material;

[0033] Note: The new core-shell modifier must be added after the liquid plasticizer has been completely absorbed by the polyvinyl chloride resin. The plasticizer, polyvinyl chloride resin and the new core-shell modifier cannot be mixed at the same time. Because when added at the same time, the new core-shell modifier will preferentially absorb the plasticizer, resulting in an uneven mixture.

[0034] S2: The mixed material is placed at room temperature for aging for 12 to 24 hours, and then input into a twin-screw extruder for plasticization and extrusion. After vacuum shaping, folding, pulling, heating, winding and cutting, a tightly fitting non-excavation repair material is obtained.

[0035] Preferably, the novel core-shell modifier is prepared by emulsion polymerization, comprising the following steps:

[0036] Add 100g of deionized water, 0.5g of emulsifier sodium dodecyl sulfate (SDS) and 20g of styrene-butadiene latex into a container and stir for 30min to obtain a core layer pre-emulsion; take another container and dissolve 0.2g of initiator potassium polysulfate (KPS) in 50g of deionized water to obtain an initiator aqueous solution; add 30g of deionized water and 1 / 3 of the prepared core layer pre-emulsion into a 500ml four-necked flask equipped with a stirrer, a thermometer, a reflux condenser and a constant pressure funnel, stir and heat to 60°C, then add 0.3g of emulsifier SDS and 1 / 3 of the initiator aqueous solution , react at a constant temperature for about 30 minutes, slowly add the remaining core layer pre-emulsion and 1 / 3 of the initiator aqueous solution, raise the temperature to 80°C, and react at a constant temperature for 60 minutes. Then, use a constant pressure dropping funnel to add 5g of butadiene, 10g of acrylonitrile and the remaining initiator aqueous solution to the reaction container. Add it over 1 to 1.5 hours. Continue to react for 2 to 4 hours, cool to room temperature, adjust the pH value to 7 to 9 with ammonia water, pour the reaction solution into another container, add 5 to 10wt% of MgSO4 aqueous solution, and obtain a new core-shell modifier in white powder form by demulsification, filtration, washing and drying.

[0037] Preferably, the polyvinyl chloride resin is composed of SG-3 type resin and SG-5 type resin in a weight ratio of 1: 1. The use of SG-3 resin and SG-5 resin in a proportioned compound can ensure material strength and take into account processing performance, and is more suitable for the production of high-performance pipes.

[0038] Preferably, the lubricant is one or more of PE wax, calcium stearate, and oxidized polyethylene wax;

[0039] The plasticizer is dioctyl terephthalate or epoxidized soybean oil. Based on 100 parts by weight of the polyvinyl chloride resin, the amount of the plasticizer is 3 to 10 parts, preferably 3 to 5 parts. If the amount of the plasticizer is too low, it is difficult to play a plasticizing role. On the contrary, if the content of the plasticizer is higher than 10 parts, the strength of the material is insufficient.

[0040] The above implementation has the advantages of:

[0041] The above scheme of the present invention has the following beneficial effects:

[0042] (1) When the material prepared by emulsion polymerization with a new core-shell modifier as the toughening agent and having styrene-butadiene rubber as the core and butadiene-acrylonitrile copolymer as the shell is impacted, the rubber particles in the core layer undergo elastic deformation, which can significantly improve the toughness of the material. The copolymer in the shell layer has good compatibility with the PVC matrix, so that it can be evenly dispersed in the PVC matrix to form a three-dimensional network cross-linked structure. In addition, due to the rigidity of the butadiene-acrylonitrile polymer itself, the material is endowed with good rigidity.

[0043] (2) Different from the currently used CPE, ACR, polyurethane, polyolefin and other elastomers as toughening materials for PVC, these low modulus elastomers will sacrifice a certain modulus and rigidity of the material while achieving toughening. The self-made new core-shell modifier is introduced into PVC by blending and melt extrusion. The self-made new core-shell modifier has good compatibility with the PVC matrix. The modified PVC liner pipe not only obtains good toughness, but also the rigidity of the material can be well guaranteed, so that it can better meet the application requirements. The liner pipe has better thermal expansion and ductility, and can achieve 150% or more expansion construction, so that a single-caliber liner pipe can adapt to more calibers of original pipes (for example: DN280 liner pipe can fit tightly to repair DN450 caliber damaged pipes), and can still maintain a high ring stiffness (≥8KN / m after expansion construction). 2 ), which has better application effect when the pipe to be repaired changes its diameter.

[0044] (3) The overall process of the preparation method of the present invention is mature, simple and easy to operate, the equipment can operate continuously, and it can meet the needs of mass production and manufacturing, and has good application prospects.

[0045] The following will describe the invention through specific embodiments.

[0046] Example 1

[0047] A process for preparing a close-fitting trenchless repair material comprises the following steps:

[0048] 1) 100 parts of polyvinyl chloride resin, 5 parts of nano calcium carbonate, 2 parts of calcium zinc stabilizer, and 0.2 parts of PE wax are added into a high-speed mixer, and when the temperature rises to 70-80° C., 3 parts of dioctyl terephthalate are added, and the mixing is continued until the temperature reaches 110° C., 5 parts of a self-made novel core-shell modifier are added, and the mixing is continued until the temperature reaches 130-135° C., and the hot mixed material is transferred into a cold mixing device for mixing and cooling until the temperature is below 50° C., and then discharged and sieved to obtain a mixed material;

[0049] 2) The mixed material in step 1 is placed at room temperature for aging for 12 to 24 hours, and then input into a twin-screw extruder for plasticization and extrusion, and a tightly fitting trenchless repair PVC liner pipe is obtained through vacuum shaping, folding, pulling, heating, winding, and cutting.

[0050] The novel core-shell modifier is prepared by emulsion polymerization, which comprises the following steps:

[0051] Add 100g of deionized water, 0.5g of emulsifier sodium dodecyl sulfate (SDS) and 20g of styrene-butadiene latex into a container and stir for 30min to obtain a core layer pre-emulsion; take another container and dissolve 0.2g of initiator potassium polysulfate (KPS) in 50g of deionized water to obtain an initiator aqueous solution; add 30g of deionized water and 1 / 3 of the prepared core layer pre-emulsion into a 500ml four-necked flask equipped with a stirrer, a thermometer, a reflux condenser and a constant pressure funnel, stir and heat to 60°C, then add 0.3g of emulsifier SDS and 1 / 3 of the initiator aqueous solution , react at a constant temperature for about 30 minutes, slowly add the remaining core layer pre-emulsion and 1 / 3 of the initiator aqueous solution, raise the temperature to 80°C, and react at a constant temperature for 60 minutes. Then, use a constant pressure dropping funnel to add 5g of butadiene, 10g of acrylonitrile and the remaining initiator aqueous solution to the reaction container. Add it over 1 to 1.5 hours. Continue to react for 2 to 4 hours, cool to room temperature, adjust the pH value to 7 to 9 with ammonia water, pour the reaction solution into another container, add 5 to 10wt% of MgSO4 aqueous solution, and obtain a new core-shell modifier in white powder form by demulsification, filtration, washing and drying.

[0052] Example 2

[0053] The difference from Example 1 is that the amount of the new core-shell modifier is replaced with 6 parts, and the other preparation steps and parameters are the same as those in Example 1.

[0054] Example 3

[0055] The difference from Example 1 is that the amount of nano calcium carbonate is replaced by 8 parts, the amount of the new core-shell modifier is replaced by 8 parts, the amount of the calcium zinc stabilizer is replaced by 3 parts, and the amount of dioctyl terephthalate is replaced by 4 parts. The remaining preparation steps and parameters are the same as those in Example 1.

[0056] Example 4

[0057] The difference from Example 1 is that the amount of nano calcium carbonate is replaced by 10 parts, the amount of the new core-shell modifier is replaced by 10 parts, the amount of the calcium zinc stabilizer is replaced by 3 parts, and the amount of dioctyl terephthalate is replaced by 4 parts. The remaining preparation steps and parameters are the same as those in Example 1.

[0058] Comparative Example 1

[0059] The difference from Example 1 is that the amount of the new core-shell modifier is replaced with 3 parts, and the other preparation steps and parameters are the same as those in Example 1.

[0060] Comparative Example 2

[0061] The difference from Example 1 is that the amount of the new core-shell modifier is replaced with 12 parts, and the other preparation steps and parameters are the same as those in Example 1.

[0062] Comparative Example 3

[0063] The difference from Example 1 is that CPE is used to replace the new core-shell modifier, and the remaining preparation steps and parameters are the same as those in Example 1.

[0064] Comparative Example 4

[0065] The difference from Example 1 is that polyurethane is used to replace the new core-shell modifier, and the remaining preparation steps and parameters are the same as those in Example 1.

[0066] The compositions of the above embodiments and comparative examples can be found in Table 1 below.

[0067]

[0068] After the closely fitting trenchless repair materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were restored to a circular shape without expansion and diameter change, the tensile strength, elongation at break, bending performance and ring stiffness were tested according to GB / T 8804, GB / T 9341 and GB / T 9647, respectively. The results are shown in Table 2:

[0069] Table 2 Test performance table of materials of Examples 1 to 4 and Comparative Examples 1 to 4

[0070]

[0071] After the tightly fitting PVC liner pipes for trenchless repair prepared in Examples 1-4 and Comparative Examples 1-4 were restored to a circular shape and expanded by 150%, a ring stiffness test was performed according to GB / T 9647. The results are shown in Table 3:

[0072] Table 3 Test performance of materials after expansion of Examples 1 to 4 and Comparative Examples 1 to 4

[0073]

[0074]

[0075] As can be seen from Table 2 and Table 3 above, the comparison between Examples 1 to 4 and Comparative Examples 3 to 4 shows that the preparation method provided by the present application uses a self-made new core-shell modifier to prepare a tightly fitting PVC liner pipe for trenchless repair. Its elongation at break, bending modulus, ring stiffness and other properties are significantly better than those of the control group, and the ring stiffness of the pipe after expansion can still be maintained at a high level, which is significantly better than the control group. Among them, Control Groups 3 to 4 did not add a self-made new core-shell modifier but used traditional CPE and polyurethane toughening modification. It can be seen from Examples 1 to 4 and Comparative Examples 1 to 2 that the different raw material ratios for preparing PVC liner pipes will result in different performance indicators of the corresponding materials, which cannot be set arbitrarily.

[0076] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A close-fitting trenchless repair material, characterized in that: The invention comprises the following components by weight: 100 parts of polyvinyl chloride resin, 5 to 10 parts of nano calcium carbonate, 5 to 10 parts of novel core-shell modifier, 2 to 4 parts of calcium zinc stabilizer, 0.2 to 0.4 parts of lubricant and 3 to 10 parts of plasticizer.

2. The close-fitting trenchless repair material according to claim 1, characterized in that: The novel core-shell modifier is prepared by emulsion polymerization, with styrene-butadiene rubber as the core and butadiene-acrylonitrile copolymer as the shell.

3. The close-fitting trenchless repair material according to claim 1, characterized in that: The polyvinyl chloride resin is composed of SG-3 type resin and SG-5 type resin in a weight ratio of 1:

1.

4. The close-fitting trenchless repair material according to claim 1, characterized in that: The lubricant is at least one of PE wax, calcium stearate and oxidized polyethylene wax.

5. The close-fitting trenchless repair material according to claim 1, characterized in that: The plasticizer is dioctyl terephthalate or epoxidized soybean oil.

6. A method for preparing a close-fitting trenchless repair material, characterized in that: The steps include: S1: According to the formula, weigh polyvinyl chloride resin, nano calcium carbonate, calcium zinc stabilizer, and lubricant, add them into a high-speed mixer for mixing, heat up, add plasticizer and mix; heat up, add new core-shell modifier and mix, transfer the hot mixture into a cold mixing equipment for mixing and cooling, discharge, sieve, and obtain a mixture; S2: The mixed material is left to mature at room temperature, and then input into a twin-screw extruder for plasticization and extrusion. After vacuum shaping, folding, pulling, heating, winding and cutting, a tightly fitting non-excavation repair material is obtained.

7. The method for preparing a close-fitting trenchless repair material according to claim 6, characterized in that: In step S1, a plasticizer is added when the temperature rises to 70-80°C; a novel core-shell modifier is added when the temperature rises to 110°C; and when the temperature reaches 130-135°C, the hot mixed material is transferred to a cold mixing device for mixing and cooling until the temperature is below 50°C and discharged.

8. The method for preparing a close-fitting trenchless repair material according to claim 6, characterized in that: In step S2, the aging time is 12 to 24 hours.

9. The method for preparing a close-fitting trenchless repair material according to claim 6, characterized in that: The preparation method of the novel core-shell modifier comprises the following steps: Deionized water, emulsifier and styrene-butadiene latex are stirred to obtain a core layer pre-emulsion; Dissolving the initiator in deionized water to obtain an initiator aqueous solution; Add deionized water and 1 / 3 of the core layer pre-emulsion into a four-necked flask, stir and heat, then add an emulsifier and 1 / 3 of the initiator aqueous solution, and react at a constant temperature; slowly dropwise add the remaining core layer pre-emulsion and 1 / 3 of the initiator aqueous solution, heat and react at a constant temperature; dropwise add butadiene, acrylonitrile and the remaining initiator aqueous solution, react, cool to room temperature, adjust the pH value with ammonia water, and obtain a mixed solution; A manganese sulfate aqueous solution is added to the mixed solution, and the mixture is demulsified, filtered, washed, and dried to obtain the product.

10. The method for preparing a close-fitting trenchless repair material according to claim 9, characterized in that: The emulsifier is sodium dodecyl sulfate; the initiator is potassium polysulfate.