High-magnetic-degree mold pressing material, button with fiber effect and preparation method of button

By using amino molding powder, fiber particles and other materials, combined with baking, molding and polishing, the problem that buttons cannot achieve high magnetic and fiber feel in the prior art is solved, and a high magnetic and fiber feel is prepared. The effect button has good heat, sun and fire resistance.

CN118931220APending Publication Date: 2024-11-12ZHEJIANG WEIXING IND DEV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411145174.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing resin molded buttons cannot achieve high magnetic and fiber-sensitive effects, and when adding plant fiber materials, they cannot show high magnetic and fiber-sensitive effects.

Method used

Using amino molding powder, fiber particles, formaldehyde reactive resin liquid, water, methylglycerol, titanium dioxide and organic pigments, it is formed by extruding into sheet-like materials, baking, molding, polishing and fleece-sensitive treatment. High magnetic buttons with fiber-filled feel.

Benefits of technology

The prepared buttons have high magnetic, high temperature resistance, no deformation, outdoor sun resistance, fire resistance, flame retardant, etc., and show high magnetic and fiber-sensitive effects. They can be mass-produced, with low cost, and are visually different from Other resin and plastic buttons.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005002381110000011
    Figure BDA0005002381110000011
  • Figure BDA0005002381110000021
    Figure BDA0005002381110000021
  • Figure BDA0005002381110000031
    Figure BDA0005002381110000031
Patent Text Reader

Abstract

The invention provides a high-magnetic molding material and a button with a fiber effect. The high-magnetic molding material is prepared from the following raw materials in parts by weight: 53-58 parts of amino molding powder; the paint is prepared from, by weight, 0-15 parts of fiber particles, 22-26 parts of formaldehyde reaction type resin liquid, 8-10 parts of water, 0.1-0.2 part of methyl glycerin, 1-1.5 parts of titanium dioxide and 0.5-1 part of organic pigment. The button provided by the invention is prepared by taking the amino molding powder, the fiber particles and the formaldehyde reaction type resin liquid as main materials and adding auxiliary materials such as the organic pigment for compatibility, shows high magnetic degree and has a fiber velvet feeling effect. The formed finished product button can resist high temperature of 120 DEG C, does not deform after 24 hours and does not crack after being exposed to the sun for 30 days outdoors, and the whole material of the button has the properties of fire prevention, flame retardance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of button technology, and in particular relates to a high-magneticity molded material and a fiber-effect button and a preparation method thereof. Background Art

[0002] In my country, buttons can be traced back to 1,800 years ago. The earliest buttons were mainly stone buttons, wooden buttons, and shell buttons. Later, they developed into ribbon buttons and knotted buttons made of cloth.

[0003] There are many materials for making buttons: such as metal, plastic, resin, fruit shell, horn, bamboo, wood, shell, etc. With the rise of the global recycling concept initiated by the European Union in recent years, and the growing global demand for environmental friendliness, buttons and clothing are an important recycling concept for recycling and reuse. At the same time, after recycling and remanufacturing, they must have the aesthetic beauty and performance that can match the fabric, so that they will be more popular with domestic and foreign customers.

[0004] At present, the buttons made by resin molding are first poured into the centrifuge with unsaturated polyester resin liquid, and then the resin is formed after semi-gelatinization to form a soft gel, and then put into the vertical molding machine and molded, and then the blank with molded concave positions is obtained. After shaping and polishing, a button with a hard texture and a strong plastic feeling can be obtained. Due to material and process reasons, the front of the button is mostly made of translucent and patterned unsaturated polyester material, with light color and texture. Therefore, the obtained button feels hard, the overall texture is crystal clear, and the plastic texture is obvious. It is impossible to achieve high magnetic colors and add plant fiber materials for compatibility, and it is impossible to present the effects of high magnetic degree and fiber feeling and the extreme velvety full matte.

[0005] Therefore, providing a button that can present high magnetic properties and fiber-like effects becomes a problem to be solved. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide a high magnetic degree molded material and a fiber effect button and a preparation method thereof. The button provided by the present invention can present high magnetic degree and fiber effect.

[0007] The present invention provides a high-magnetic molded material and a fiber-effect button, and the raw materials for preparing the material include:

[0008]

[0009]

[0010] Preferably, the amino molding powder is selected from amino molding powder material extracted from bamboo.

[0011] Preferably, the fiber particles are selected from one or more of sawdust powder, corn cob powder and straw powder;

[0012] The particle size of the fiber particles is 60 to 80 meshes.

[0013] Preferably, the fiber particles are used in an amount of 8 to 15 parts by weight.

[0014] The present invention also provides a method for preparing the button, comprising the following steps:

[0015] A) mixing amino molding powder, fiber particles, formaldehyde reactive resin liquid, water, methyl glycerol, titanium dioxide, and organic pigment and extruding the mixture to obtain a sheet material;

[0016] B) forming the sheet material into blanks and then baking the blanks to obtain dried blanks;

[0017] C) subjecting the dried blank to compression molding to obtain a button blank;

[0018] D) polishing the button blank, performing a velvet treatment, and cleaning the button blank to obtain a button.

[0019] Preferably, the method for baking the dough is:

[0020] The blank obtained after the blank making is baked at 50-55° C. for 14-16 hours, then turned over and baked for another 2-4 hours.

[0021] Preferably, the compression molding temperature is 140-147° C. and the time is 70-120 seconds.

[0022] Preferably, the polishing method comprises:

[0023] After removing the burrs on the corners, shapes and edges of the button blank, it is polished by water roller.

[0024] Preferably, the acidification treatment liquid used for the velvet treatment comprises:

[0025] 100 parts by weight of water, 2 to 3 parts by weight of sodium sulfonate and 8 to 12 parts by weight of hydrochloric acid;

[0026] The velvet treatment lasts for 10 to 15 minutes.

[0027] Preferably, the cleaning is performed by soaking in water for 25 to 30 minutes.

[0028] Compared with the prior art, the present invention provides a high magnetic molding material and fiber effect buttons, and the raw materials for preparation include: 53-58 parts by weight of amino molding powder; 0-15 parts by weight of fiber particles, 22-26 parts by weight of formaldehyde reaction type resin liquid, 8-10 parts by weight of water, 0.1-0.2 parts by weight of methyl glycerol, 1-1.5 parts by weight of titanium dioxide, and 0.5-1 parts by weight of organic pigment. The buttons provided by the present invention are made of amino molding powder, fiber particles and formaldehyde reaction type resin liquid as the main materials, and are matched with auxiliary materials such as organic pigments, showing high magnetic properties and having a fiber velvety effect. The finished button can withstand high temperatures of 120°C, does not deform for 24 hours, and does not crack in outdoor exposure for 30 days. The overall button material has properties such as fire retardancy. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a photo of the button prepared in Example 1;

[0030] Figure 2 This is a photo of the button prepared in Example 1;

[0031] Figure 3 This is a photo of the button prepared in Example 2;

[0032] Figure 4 This is a photo of the button prepared in Example 2;

[0033] Figure 5 This is a photo of the button prepared in Example 3;

[0034] Figure 6 This is a photo of the buttons prepared in Example 3. DETAILED DESCRIPTION

[0035] The present invention provides a high-magnetic molded material and a fiber-effect button, and the raw materials for preparing the material include:

[0036]

[0037] The raw materials for preparing the high magnetic molding material and fiber effect buttons provided by the present invention include 53-58 parts by weight of amino molding powder, which can be 53, 53.5, 54, 54.5, 55, 55.5, 56, 56.5, 57, 57.5, 58, or any value between 53 and 58 parts by weight. The amino molding powder is selected from modified bamboo amino molding powder, which is an amino molding powder material extracted from bamboo.

[0038] The raw materials for preparing the high magnetic molding material and fiber effect buttons provided by the present invention also include 0 to 15 parts by weight of fiber particles, that is, the present invention can add fiber particles to the buttons or not. When the buttons need to present a particle effect, the amount of the fiber particles is 8 to 15 parts by weight, which can be 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, or any value between 8 and 15 parts by weight. The fiber particles are selected from one or more of sawdust powder, corn cob powder and straw powder; the particle size of the fiber particles is 60 to 80 meshes.

[0039] The raw materials for preparing the high magnetic molding material and fiber effect buttons provided by the present invention also include 22 to 26 parts by weight of formaldehyde reactive resin liquid, which can be 22, 22.5, 23, 23.5, 24, 24.5, 25, 25.5, 26, or any value between 22 and 26 parts by weight.

[0040] The raw materials for preparing the high magnetic molding material and fiber effect buttons provided by the present invention also include 8 to 10 parts by weight of water, which may be 8, 8.5, 9, 9.5, 10, or any value between 8 and 10 parts by weight.

[0041] The raw materials for preparing the high magnetic molding material and fiber effect buttons provided by the present invention also include 0.1-0.2 parts by weight of methyl glycerol, which can be 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, or any value between 0.1 and 0.2 parts by weight.

[0042] The raw materials for preparing the high magnetic molding material and fiber effect buttons provided by the present invention also include 1 to 1.5 parts by weight of titanium dioxide, which can be 1, 1.1, 1.2, 1.3, 1.4, 1.5, or any value between 1 and 1.5 parts by weight.

[0043] The raw materials for preparing the high magnetic molding material and fiber effect buttons provided by the present invention further include 0.5 to 1 parts by weight of organic pigment, which can be 0.5, 0.6, 0.7, 0.8, 0.9, 1, or any value between 0.5 and 1 parts by weight. The present invention has no special restrictions on the specific type of the organic pigment, and the color of the organic pigment can be selected according to the needs. It can be one or more of red, yellow, blue, and black.

[0044] The high-magneticity molded material and fiber-effect button provided by the invention have high magnetism and fiber effect.

[0045] The present invention also provides a method for preparing the above-mentioned button, characterized in that it comprises the following steps:

[0046] A) mixing amino molding powder, fiber particles, formaldehyde reactive resin liquid, water, methyl glycerol, titanium dioxide, and organic pigment and extruding the mixture to obtain a sheet material;

[0047] B) forming the sheet material into blanks and then baking the blanks to obtain dried blanks;

[0048] C) subjecting the dried blank to compression molding to obtain a button blank;

[0049] D) polishing the button blank, performing a velvet treatment, and cleaning the button blank to obtain a button.

[0050] The present invention uses amino molding powder as the main material, adds various fiber particles or no fiber particles (after adding fiber particles, the button shows a particle effect, and without fiber particles, the button shows a monochrome effect), methyl glycerol and titanium dioxide, and then adds organic pigments to adjust the color. After the separation is evenly mixed by a grinding device, a water-soluble reactive resin solution is added, and after being evenly stirred by a mixer, it is taken out for sheet extrusion and put into a blank extruder for blanking. Then, after the blank is baked, the blank is formed, and then the button is shaped and polished, and finally the surface is fully matte velvet through acidification treatment to obtain the required high magnetic fiber effect button.

[0051] In the present invention, there are two ways to prepare buttons: the button shape can be directly pressed by a mold button shape, or the button shape can be made by pressing a mold blank.

[0052] Specifically, the present invention firstly puts the raw materials into a mixer, mixes them evenly, and then puts them into a sheet extruder to extrude them into sheets to obtain sheet materials, wherein the thickness of the sheet materials can be adjusted according to the thickness requirements of the product.

[0053] Then, the sheet material is blanked. Specifically, the sheet material is put into a blank extruder and cut into blanks of a desired shape.

[0054] Then the blank is baked, wherein the method of baking the blank is:

[0055] The blank obtained after the blank making is baked at 50-55° C. for 14-16 hours, then turned over and baked for another 2-4 hours.

[0056] The baking temperature may be 50, 51, 52, 53, 54, 55, or any value between 50 and 55° C. The baking is to volatilize the moisture in the blank.

[0057] Then, the obtained dried blank is subjected to compression molding to obtain a button blank. The compression molding temperature is 140-147°C, which can be 140, 141, 142, 143, 144, 145, 146, 147, or any value between 140-147°C, and the time is 70-120s, which can be 70, 80, 90, 100, 110, 120, or any value between 70-120s. Preferably, the dried blank is placed in a mold vulcanizing molding machine that has been equipped with a specific required shape and blank for compression molding.

[0058] The shape of the button is formed by combining the function of the mold, and can be formed into various required shapes, and the required shape is formed by cutting through special shaping equipment.

[0059] Next, the button blank is taken out and cut into pieces for polishing, wherein the polishing method comprises:

[0060] After removing the burrs on the corners, shapes and edges of the button blank, it is polished by water roller.

[0061] Then, the polished button blank is subjected to a velvet treatment, wherein the acidified treatment liquid used for the velvet treatment comprises:

[0062] 100 parts by weight of water, 2 to 3 parts by weight of sodium sulfonate and 8 to 12 parts by weight of hydrochloric acid.

[0063] Specifically, based on 100 parts by weight of water, the treatment liquid includes 2 to 3 parts by weight of sodium sulfonate, which can be 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, or any value between 2 and 3 parts by weight.

[0064] Based on 100 parts by weight of water, the treatment liquid also includes 8 to 12 parts by weight of hydrochloric acid, which can be 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, or any value between 8 and 12 parts by weight.

[0065] The polished button blank is placed in a treatment liquid for velvet treatment, wherein the velvet treatment time is 10 to 15 minutes, which can be 10, 11, 12, 13, 14, 15, or any value between 10 and 15 minutes.

[0066] After the velvet treatment, the button surface as a whole has a slight velvety feel and a whitened appearance.

[0067] Finally, the button blanks treated with velvet are cleaned by soaking in water for 25 to 30 minutes.

[0068] The button provided by the present invention is synthesized from amino molding powder material, fiber particles, formaldehyde reaction type resin liquid and other raw materials through modified synthesis. After the thermoplastic effect of hot pressing equipment, the whole material is quickly plasticized and formed under the action of high temperature, and a blank and button meeting a certain standard hardness are formed. At the same time, in order to achieve excellent blank performance, a special molding machine can be used to cut the round blank to form a required shape button, and it has high magnetic properties and fiber velvet effect.

[0069] The present invention makes a breakthrough in the manufacturing of raw materials combined with processing technology. The product is formed once, then formed twice and chemically treated, presenting a new texture:

[0070] 1. The synthetic use of raw materials makes a breakthrough in the original button molding method, presenting a new texture product on the die-cast buttons;

[0071] 2. In terms of production efficiency, it can be mass-produced, with batch post-processing modeling and chemical treatment texture, which has the advantages of high output efficiency, low cost and high profit;

[0072] 3. In terms of visual effects, it directly presents the high magnetic texture, the embedded effect of fiber particles, and the velvety (semi-gloss, matte) whitening texture on the surface, which visually gives people a clear difference from other resin buttons and plastic buttons.

[0073] In order to further understand the present invention, the high magnetic molded material and fiber effect button and the preparation method thereof provided by the present invention are described below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0074] In the following examples, the amino molding powder is commercially available amino molding powder, specifically amino molding powder extracted from bamboo, purchased from Changzhou Qiaoer Plastic Co., Ltd.;

[0075] The fiber particles are scrap powder particles produced by recycling wood and straw processing plants, and the particle size is 60 to 80 meshes;

[0076] The formaldehyde-reactive resin liquid is a commercially available formaldehyde-reactive resin liquid purchased from Zhejiang Jiashan Hongxin Chemical Factory;

[0077] The methyl glycerol is a commercially available medical grade raw material;

[0078] The titanium dioxide and organic pigment are commercially available raw materials.

[0079] Embodiment 1:

[0080] 1. The formula is as follows:

[0081]

[0082] 2. Preparation process

[0083] Step 1: Put all the above raw materials into a blender according to the proportion, mix them evenly and then put them into a sheet extruder to extrude them into sheets;

[0084] Step 2: Put the above sheet material into the extruder, cut it into round blanks, and put it into a specific oven for water volatilization and semi-solidification. The temperature is set to 50 degrees Celsius for 14 hours, and the blanks are turned over once, and then baked for 2 hours;

[0085] Step 3: Place the dried blank into a vulcanizing molding machine with a mold having a specific shape and blank, and perform molding at a molding temperature of 140°C for 70 seconds, exhaust twice, and press into button blanks and semi-finished buttons;

[0086] Step 4: Take the button blanks, polish them and remove burrs from the edges and corners to obtain polished button blanks and semi-finished buttons;

[0087] Step 5: After shaping and scraping the burrs of the button blanks and semi-finished buttons, they are subjected to water tumbling and polishing treatment;

[0088] Step 6: Prepare the acid treatment solution. The formula is as follows:

[0089] Water 100 parts by weight

[0090] Sodium sulfonate 2.0 parts by weight

[0091] 8.0 parts by weight of hydrochloric acid

[0092] Step 7: Soak the polished buttons in the prepared solution for 10 minutes, until the surface of the buttons has a slight velvety feeling and a whitened appearance, which is the desired effect. Wash with clean water and soak for 30 minutes, then dehydrate and dry in a centrifuge to obtain the finished buttons.

[0093] See also Figure 1 and Figure 2 , Figure 1 This is a photo of the buttons prepared in Example 1. Figure 2 This is a photo of the buttons prepared in Example 1. Figure 1 and Figure 2 The prepared buttons are different only in the color of the organic pigment, and the other formulas and processes are the same.

[0094] Embodiment 2:

[0095] 1. The formula is as follows:

[0096]

[0097] 2. Preparation process

[0098] Step 1: Put all the above raw materials into a blender according to the proportion, mix them evenly and then put them into a sheet extruder to extrude them into sheets;

[0099] Step 2: Put the above sheet material into the extruder, cut it into round blanks, and put it into a specific oven for water volatilization and semi-solidification. The temperature is set to 55 degrees Celsius for 16 hours, and the blanks are turned over once, and then baked for 3 hours;

[0100] Step 3: Place the dried blank into a vulcanizing molding machine with a mold having a specific shape and blank, and perform molding at a molding temperature of 145°C for 100 seconds, exhaust twice, and press into button blanks and semi-finished buttons;

[0101] Step 4: Take the button blanks, polish them and remove burrs from the edges and corners to obtain polished button blanks and semi-finished buttons;

[0102] Step 5: After shaping and scraping the burrs of the button blanks and semi-finished buttons, they are subjected to water tumbling and polishing treatment;

[0103] Step 6: Prepare the acid treatment solution. The formula is as follows:

[0104] Water 100 parts by weight

[0105] Sodium sulfonate 3.0 parts by weight

[0106] 12 parts by weight of hydrochloric acid

[0107] Step 7: Soak the polished buttons in the prepared solution for 13 minutes, until the surface of the buttons has a slight velvety feeling and a whitened appearance, which is the desired effect. Wash with clean water and soak for 30 minutes, then dehydrate and dry in a centrifuge to obtain the finished buttons.

[0108] See also Figure 3 and Figure 4 , Figure 3 This is a photo of the button prepared in Example 2 (no fiber particles are added, i.e., the amount of fiber particles is 0 parts by weight). Figure 4 This is a photograph of the buttons prepared in Example 2 (fiber particles were added, i.e., the amount of fiber particles was 10 parts by weight).

[0109] Embodiment 3:

[0110] 1. The formula is as follows:

[0111]

[0112] 2. Preparation process

[0113] Step 1: Put all the above raw materials into a blender according to the proportion, mix them evenly and then put them into a sheet extruder to extrude them into sheets;

[0114] Step 2: Put the above sheet material into the extruder, cut it into round blanks, and put it into a specific oven for water volatilization and semi-solidification. The temperature is set to 53 degrees Celsius for 15 hours, and the blanks are turned over once, and then baked for another 4 hours;

[0115] Step 3: Place the dried blank into a vulcanizing molding machine with a mold having a specific shape and blank, and perform molding at a molding temperature of 147°C for 120 seconds, exhaust twice, and press into button blanks and semi-finished buttons;

[0116] Step 4: Take the button blanks, polish them and remove burrs from the edges and corners to obtain polished button blanks and semi-finished buttons;

[0117] Step 5: After shaping and scraping the burrs of the button blanks and semi-finished buttons, they are subjected to water tumbling and polishing treatment;

[0118] Step 6: Prepare the acid treatment solution. The formula is as follows:

[0119] Water 100 parts by weight

[0120] Sodium sulfonate 2.0 parts by weight

[0121] 8.0 parts by weight of hydrochloric acid

[0122] Step 7: Soak the polished buttons in the prepared solution for 13 minutes, until the surface of the buttons has a slight velvety feeling and a whitened appearance, which is the desired effect. Wash with clean water and soak for 30 minutes, then dehydrate and dry in a centrifuge to obtain the finished buttons.

[0123] See also Figure 5 and Figure 6 , Figure 5 This is a photo of the button prepared in Example 3 (no fiber particles are added, i.e., the amount of fiber particles is 0 parts by weight). Figure 6 This is a photo of the button prepared in Example 3 (adding fiber particles, i.e., the amount of fiber particles is 10 parts by weight). And, according to the needs, Figure 5 and Figure 6 The buttons used are of different shapes.

[0124] Test Case

[0125] The finished buttons of Examples 1 to 3 were subjected to performance tests:

[0126] Tested according to the international standard ISO 105-C06-2010 "Colour fastness to domestic and commercial washing", the colour fastness to washing must be ≥ 4.5;

[0127] Tested according to the international standard ISO 105-D01-2010 "Color fastness to dry cleaning of textiles", the color fastness to dry cleaning should be ≥ 4.5;

[0128] Tested according to the international standard ISO 105-X11-1994 "Color fastness to hot pressing of textiles", the color fastness to ironing should be ≥ 4.5;

[0129] The test is carried out according to Method A specified in GB / T2408-2021 "Horizontal and Vertical Methods for Determination of Combustion Performance of Plastics" and meets the HB level of combustion performance.

[0130] High temperature resistance: Use an electric oven, set the temperature to 120℃, and time for 24 hours. Figures 1 to 6 5 buttons of each type) were laid flat on a stainless steel plate for processing and judged whether they were deformed. After testing, all 30 buttons were not deformed and had good high temperature resistance.

[0131] Sun resistance: 15 buttons were pasted on the front and back of a cardboard, and then placed outdoors in direct sunlight for 72 hours to determine whether there were any cracks. After testing, all buttons were found to be free of cracks, showing good sun resistance.

[0132] Comparative Example 1

[0133] Based on Example 1, steps 1 to 5 are the same.

[0134] Step 6: Prepare the acid treatment solution. The formula is as follows:

[0135] Water 100 parts by weight

[0136] Sodium sulfonate 2.0 parts by weight

[0137] Nitric acid 8.0 parts by weight

[0138] Step 7: Soak the polished buttons in a solution replaced with nitric acid for 10 minutes. Obvious corrosion occurs on the surface of the buttons, and the surface is relatively rough, which does not match the velvety texture.

[0139] Comparative Example 2

[0140] On the basis of Example 1, steps 1 to 5 are the same, and step 6 is changed

[0141] Step 6: Prepare the acid treatment solution. The formula is as follows:

[0142] Water 100 parts by weight

[0143] 2.0 parts by weight of sodium hydroxide

[0144] 8.0 parts by weight of hydrochloric acid

[0145] Step 7: Soak the polished buttons in a solution replaced with sodium hydroxide for 13 minutes. The surface texture of the buttons has no obvious change and is the same as after polishing, without any velvety feeling of being slightly corroded.

[0146] Comparative Example 3

[0147] Based on Example 2, steps 1 to 5 are the same, and step 6 is changed

[0148] Step 6: Prepare the acid treatment solution. The formula is as follows:

[0149] Water 100 parts by weight

[0150] 3.0 parts by weight of sodium hydroxide

[0151] Acetic acid 12 parts by weight

[0152] Step 7: Soak the polished buttons in the treatment solution for 15 minutes. There is no obvious change in the surface texture of the buttons, which is the same as the texture after polishing, and there is no velvety texture caused by slight corrosion.

[0153] Comparative Example 4

[0154] 1. The formula is as follows:

[0155]

[0156] 2. Preparation process

[0157] Step 1: Put all the above raw materials into a blender according to the proportion, mix them evenly and then put them into a sheet extruder to extrude them into sheets;

[0158] Step 2: Put the above sheet material into the extruder, cut it into round blanks, and put it into a specific oven for water volatilization and semi-solidification. The temperature is set to 70 degrees Celsius for 14 hours, and the blanks are turned over once, and then baked for 2 hours;

[0159] Step 3: Place the dried blanks into a vulcanizing molding machine that has been equipped with a mold according to specific requirements and blanks for molding. Raise the molding temperature to 155°C for 70 seconds and exhaust twice. When pressed into button blanks and semi-finished buttons, there are many bubbles on the surface of the buttons, which do not meet the quality standards.

[0160] Comparative Example 5

[0161] 1. The formula is as follows:

[0162]

[0163] 2. Preparation process

[0164] Step 1: replace the methyl glycerol in the raw material formula of Example 3 with white oil, synthesize according to the ratio, put into a blender, stir evenly, and then put into a sheet extruder to extrude into sheets;

[0165] Step 2: Put the above sheet material into the extruder, cut it into round blanks, and put it into a specific oven for water volatilization and semi-solidification. The temperature is set to 50 degrees Celsius for 14 hours, and the blanks are turned over once, and then baked for 2 hours;

[0166] Step 3: Put the dried blank into a vulcanizing molding machine with a mold having a specific shape and blank, and perform molding. The molding temperature is 145°C, the time is 70s, and the exhaust is performed twice. When the button blank and the semi-finished button are pressed, there are many corners missing on the surface of the button, and the button is not completely cured.

[0167] Comparative Example 6

[0168] 1. The formula is as follows:

[0169]

[0170]

[0171] 2. Preparation process

[0172] Step 1: Replace the titanium dioxide in the raw material formula of Example 3 with calcium carbonate powder, synthesize according to the ratio, put into a blender, stir evenly, and then put into a sheet extruder to extrude into sheets;

[0173] Step 2: Put the above sheet material into the extruder, cut it into round blanks, and put it into a specific oven for water volatilization and semi-solidification. The temperature is set to 55 degrees Celsius for 15 hours, and the blanks are turned over once, and then baked for 2 hours;

[0174] Step 3: The dried blank is placed in a vulcanizing molding machine with a mold having a specific shape and blank, and molded at a molding temperature of 140°C for 70 seconds, and vented twice. When the button blank and semi-finished button are pressed, insoluble white particles are present on the surface of the obtained button, and the overall appearance of the button does not meet the texture standard;

[0175] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high magnetic molded material and a fiber effect button, characterized in that: The raw materials for preparation include:

2. The button according to claim 1, characterized in that: The amino molding powder is selected from amino molding powder material extracted from bamboo.

3. The button according to claim 1, characterized in that: The fiber particles are selected from one or more of sawdust powder, corn cob powder and straw powder; The particle size of the fiber particles is 60 to 80 meshes.

4. The button according to claim 1, characterized in that: The fiber particles are used in an amount of 8 to 15 parts by weight.

5. A method for preparing a button according to any one of claims 1 to 4, characterized in that: The following steps are involved: A) mixing amino molding powder, fiber particles, formaldehyde reactive resin liquid, water, methyl glycerol, titanium dioxide, and organic pigment and extruding the mixture to obtain a sheet material; B) forming the sheet material into blanks and then baking the blanks to obtain dried blanks; C) subjecting the dried blank to compression molding to obtain a button blank; D) polishing the button blank, performing a velvet treatment, and cleaning the button blank to obtain a button.

6. The preparation method according to claim 5, characterized in that: The method for baking the dough is as follows: The blank obtained after the blank making is baked at 50-55° C. for 14-16 hours, then turned over and baked for another 2-4 hours.

7. The preparation method according to claim 5, characterized in that: The temperature of the compression molding is 140-147° C., and the time is 70-120 seconds.

8. The preparation method according to claim 5, characterized in that: The polishing method comprises: After removing the burrs on the corners, shapes and edges of the button blank, it is polished by water roller.

9. The preparation method according to claim 5, characterized in that: The acidification treatment liquid used for the velvet treatment comprises: 100 parts by weight of water, 2 to 3 parts by weight of sodium sulfonate and 8 to 12 parts by weight of hydrochloric acid; The velvet treatment lasts for 10 to 15 minutes.

10. The preparation method according to claim 5, characterized in that: The cleaning is performed by soaking in water for 25 to 30 minutes.

Citation Information

Cited By

  • High-temperature-resistant flame-retardant molded button and manufacturing process thereof

    CN120535899A