Colorful stone-like coating and preparation method thereof

Through the gelation principle of guar gum and borax, the amount of borax is adjusted to control the soft and hard details of the color point, the problem of insufficient performance of existing colorful imitation stone coatings is solved, and the performance improvement and operational simplification of the coating is achieved. Enhanced.

CN118931264AActive Publication Date: 2024-11-12XIAMEN ZEHUAN BUILDING MATERIALS CO LTD

Patent Information

Application Number
CN202410537627.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-11-12
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

The existing colorful imitation stone paints have shortcomings in performance improvement, and the formulation adjustment is slow, making it difficult to effectively adjust the soft and hard details of the color dots, affecting the construction effect.

Method used

The gelation principle of guar gum and borax is adopted, and the soft and hard details of the color dots are controlled by adjusting the amount of borax, forming a stable colorful imitation stone paint, which improves the stability, water resistance and stain resistance of the paint, and Simplified formula design.

Benefits of technology

The performance improvement of colorful imitation stone paints has been achieved, and the diversity of color dot patterns and colors has been improved, and the overall performance of the paint has been improved, making the operability more convenient and has wider applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931264A_ABST
    Figure CN118931264A_ABST
Patent Text Reader

Abstract

The invention provides a colorful stone-like coating and a preparation method thereof. The colorful stone-like coating comprises a base paint, a granulation liquid and a continuous phase, the basic paint is prepared from the following components in parts by weight: 650 to 700 parts of water, 1 to 3 parts of magnesium lithium silicate, 55 to 65 parts of pigment filler, 2 to 3 parts of guar gum, 150 to 250 parts of polymer emulsion, 750 to 850 parts of quartz sand and 1 to 3 parts of borax liquid; 25-30 parts of an auxiliary agent; performances such as stability, water resistance, stain resistance and scrubbing resistance of the colorful stone-like coating can reach expected effects; the soft and hard details of the color points can achieve the expected effect only by adjusting the dosage of the borax, the operability is more convenient, and meanwhile, the performance requirements of the colorful stone-like coating are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a colorful stone-imitation coating and a preparation method thereof. Background Art

[0002] Colorful imitation stone paint is a water-based environmentally friendly series of products, created to meet the needs of today's growing exterior wall decoration paint market.

[0003] Most of the existing colorful imitation stone paints use the cross-linking reaction technology of cellulose ether and protective glue (magnesium lithium silicate) to achieve the imitation stone effect. The principle is that the hydrophilic hydroxyl groups on the cellulose molecular chain react with the magnesium lithium silicate protective glue to form a hydrogen bond hydrophobic card house structure, so that the particles will no longer fuse after separation, and the obtained colorful particles have a certain wrapping force; but due to the slow adjustability of its formula, that is, the hardness and softness of each color point must be adjusted by adjusting the entire formula system; and the performance of the obtained colorful imitation stone paint still has room for improvement.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a new colorful stone-like paint and a preparation method thereof, the performance of the colorful stone-like paint is greatly improved; the soft and hard details of the color dots can achieve the expected effect only by adjusting the amount of borax, the operability is more convenient, and the performance requirements of the colorful stone-like paint are greatly improved.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A colorful stone-like paint, comprising a base paint, a granulation liquid and a continuous phase;

[0008] The base paint comprises the following components in parts by weight:

[0009] 650-700 parts of water (e.g. 650, 660, 670, 680, 690, 700 parts),

[0010] 1-3 parts of lithium magnesium silicate (e.g. 1 part, 2 parts, 3 parts),

[0011] 55-65 parts of pigments and fillers (e.g. 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65),

[0012] 2-3 parts of guar gum (e.g. 2 parts, 2.5 parts, 3 parts),

[0013] 150-250 parts of polymer emulsion (e.g. 150 parts, 160 parts, 170 parts, 180 parts, 190 parts, 200 parts, 210 parts, 220 parts, 230 parts, 240 parts, 250 parts),

[0014] 750-850 parts of quartz sand (for example, 750 parts, 760 parts, 770 parts, 780 parts, 790 parts, 800 parts, 810 parts, 820 parts, 830 parts, 840 parts, 850 parts),

[0015] 1 to 3 parts of borax solution (e.g. 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts);

[0016] 25-30 parts of additives (e.g. 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts);

[0017] The granulation liquid comprises the following components in parts by weight:

[0018] 750-800 parts of water (e.g. 750, 760, 770, 780, 790, 800 parts),

[0019] 4-6 parts of lithium magnesium silicate (e.g. 4 parts, 5 parts, 6 parts),

[0020] 150-250 parts of borax solution (e.g. 150 parts, 160 parts, 170 parts, 180 parts, 190 parts, 200 parts, 210 parts, 220 parts, 230 parts, 240 parts, 250 parts),

[0021] 2 to 4 parts of additives (e.g. 2, 3, 4);

[0022] The continuous phase comprises the following components in parts by weight:

[0023] 250-300 parts of water (e.g. 250 parts, 260 parts, 270 parts, 280 parts, 290 parts, 300 parts),

[0024] 550-650 parts of polymer emulsion (e.g., 550 parts, 560 parts, 570 parts, 580 parts, 590 parts, 600 parts, 610 parts, 620 parts, 630 parts, 640 parts, 650 parts),

[0025] 40 to 60 parts of borax solution (e.g. 40, 45, 50, 55, 60 parts),

[0026] 60-70 parts of additives (for example, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, 70 parts).

[0027] The reason why the present invention adopts guar gum plus borax to replace the current cellulose plus protective glue is that the current cellulose and protective glue have poor water resistance. The protective glue is a mixture of artificially synthesized magnesium silicate lithium salt and metaphosphate (viscosity reducer). Glue plus borax solution can also react with gel, but it cannot form a color dot shape. The present invention does not adopt it, mainly because the glue is easy to dry. If it is exposed to the air for a long time, or in a dry environment, it is easy to evaporate the water therein, lose viscosity, and reduce the use effect of the glue, especially some water-based glues, which are more susceptible to the dry environment; and the glue is easy to stratify. Since the glue is mixed with multiple substances, part of the glue is easy to stratify. If the stratification phenomenon is too serious, the glue will lose uniformity and reduce the use effect of the glue. It should be emphasized that among the components of the present invention, the magnesium silicate lithium in the base paint and the magnesium silicate lithium in the granulation liquid are only used as thickening, suspension, isolation and adsorption functions, and are not used for cross-linking reactions.

[0028] Based on the above scheme, preferably, the mass ratio of the base paint, the granulation liquid and the continuous phase is (5-8): (1-3): (1-2).

[0029] On the basis of the above scheme, preferably, the borax liquid in the base paint, the borax liquid in the granulation liquid and the borax liquid in the continuous phase are all borax aqueous solutions; the mass concentration of borax in the borax aqueous solution is 1% to 2% (such as 1%, 1.5%, 2%). The reason for choosing borax aqueous solution is the solubility of borax and the precise control of the amount of borax. If the amount of borax is too much, it will affect the soft and hard details of the color dots and will also affect the subsequent construction effect. On the contrary, if the amount of borax is too little, the toughness of the gel is weakened. When guar gum and borax react with gel, the toughness of the gel formed is stronger when the amount of borax increases, and the toughness of the gel becomes weaker when the amount of borax decreases.

[0030] On the basis of the above scheme, preferably, the borax aqueous solution also contains a preservative, and the mass concentration of the preservative is 1% to 2% (such as 1%, 1.5%, 2%); the preservative includes at least one of 1,2-benzisothiazolin-3-one, isothiazolinone and methylisothiazolinone. The reason why a preservative needs to be added to the borax aqueous solution of the present invention is that the amount of borax needs to be preferably controlled within the scope of the present invention, but the amount of borax within the preferred range is not enough to support the antiseptic effect of the entire system, so a preservative within the preferred range of the present invention needs to be added to the borax aqueous solution.

[0031] On the basis of the above scheme, preferably, the pigment filler in the base paint includes at least one of titanium dioxide, kaolin and heavy calcium;

[0032] And / or, the polymer emulsion in the base paint includes at least one of styrene acrylic emulsion, pure acrylic emulsion, and silicone acrylic emulsion;

[0033] And / or, the additives in the base paint include the following components in parts by weight: 1-2 parts of dispersant (for example, 1 part, 2 parts), 1-2 parts of defoaming agent (for example, 1 part, 2 parts), 1-2 parts of multifunctional additive (for example, 1 part, 2 parts), 9-11 parts of antifreeze agent (for example, 9 parts, 10 parts, 11 parts), 9-11 parts of film-forming additive (for example, 9 parts, 10 parts, 11 parts), and 3-5 parts of preservative (for example, 3 parts, 4 parts, 5 parts).

[0034] On the basis of the above scheme, preferably, the auxiliary agent in the granulation liquid includes the following components in parts by weight: 1 to 2 parts (such as 1 part, 2 parts) of anti-settling agent, 1 to 3 parts (such as 1 part, 2 parts, 3 parts) of preservative;

[0035] Preferably, the anti-settling agent includes at least one of sodium carboxymethyl cellulose, a mixture of sodium carboxymethyl cellulose and xanthan gum mixed in any proportion; the preservative includes at least one of 1,2-benzisothiazolin-3-one (BIT), isothiazolinone (Kasson) and methylisothiazolinone (MIT).

[0036] And / or, the auxiliary agent in the continuous phase includes the following components in parts by weight: 1-2 parts of defoaming agent, 1-2 parts of multifunctional auxiliary agent, 15-25 parts of antifreeze agent, 35-45 parts of film-forming auxiliary agent, and 1-3 parts of preservative;

[0037] Preferably, the polymer emulsion in the continuous phase includes at least one of styrene acrylic emulsion, pure acrylic emulsion, and silicone acrylic emulsion.

[0038] On the basis of the above scheme, preferably, the dispersant in the base paint and the dispersant in the continuous phase are both at least one of anionic dispersants and non-ionic dispersants; the defoamer in the base paint and the defoamer in the continuous phase are both thick paste defoamers; the multifunctional additive in the base paint and the dispersant in the continuous phase are both 2-amino-2-methyl-1-propanol; the antifreeze in the base paint and the antifreeze in the continuous phase are both ethylene glycol; the film-forming aid in the base paint and the film-forming aid in the continuous phase are both alcohol ester dodecahydrate; the guar gum in the base paint uses hydroxypropyl guar gum; the preservative in the base paint and the preservative in the continuous phase include at least one of 1,2-benzisothiazolin-3-one, isothiazolinone and methylisothiazolinone.

[0039] In addition, the present invention also provides a method for preparing the above-mentioned colorful stone-like paint, comprising the following steps:

[0040] S1, prepare borax solution;

[0041] S2, using the borax solution prepared in step S1 to prepare a base paint, a granulation liquid and a continuous phase respectively;

[0042] S3, mixing the prepared basic paint and granulation liquid to form granules, and then adding the continuous phase and mixing evenly to obtain the colorful stone-like paint.

[0043] Based on the above scheme, preferably, in step S1, the process of preparing the borax solution specifically comprises: adding borax and a preservative to water in sequence and stirring evenly to obtain the borax solution;

[0044] And / or, in step S2, the process of preparing the base paint specifically comprises: adding lithium magnesium silicate, dispersant, pigment filler, guar gum, defoamer, and multifunctional additive to water in sequence, stirring at high speed and dispersing evenly, adding polymer emulsion, antifreeze agent, film-forming aid, preservative, and borax solution in sequence while continuing to slow down stirring, stirring at high speed again, and finally adding quartz sand and mixing evenly to obtain the base paint;

[0045] And / or, in step S2, the process of preparing the granulation liquid specifically comprises: adding lithium magnesium silicate, an anti-settling agent, a borax solution, and a preservative into water in sequence and stirring the mixture to obtain the granulation liquid;

[0046] And / or, in step S2, the process of preparing the continuous phase specifically includes: adding a defoaming agent, a multifunctional additive, an antifreeze agent, a film-forming aid, a preservative, a polymer emulsion, and a borax solution into water in sequence and stirring the mixture evenly to obtain the continuous phase.

[0047] On the basis of the above scheme, preferably, in step S1, during the process of preparing the borax solution, the stirring rate is 500-800 r / min (e.g., 500 r / min, 600 r / min, 700 r / min, 800 r / min);

[0048] And / or, in step S2, during the preparation of the base paint, the high-speed stirring rate is 1500-2000 r / min (e.g., 1500 r / min, 1600 r / min, 1700 r / min, 1800 r / min, 1900 r / min, 2000 r / min), the dispersion time is 30-40 min (e.g., 30 min, 35 min, 40 min), and the deceleration stirring rate is 500-800 r / min (e.g., 500 r / min, 600 r / min, 700 r / min, 800 r / min);

[0049] And / or, in step S2, during the process of preparing the granulation liquid, the stirring rate is 500-800 r / min (e.g., 500 r / min, 600 r / min, 700 r / min, 800 r / min);

[0050] And / or, in step S2, during the process of preparing the continuous phase, the stirring rate is 500-800 r / min (e.g., 500 r / min, 600 r / min, 700 r / min, 800 r / min).

[0051] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:

[0052] The invention adopts the gelation principle of guar gum and borax (the hydroxyl group of guar gum is combined with borax to form a borax bond), and the stability, water resistance, stain resistance and scrub resistance of the colorful stone-like paint obtained after a specific component ratio can achieve the expected effects, realize the diversity of the form and color of the color point pattern, and greatly improve the performance requirements of the colorful stone-like paint. The various performances of the colorful stone-like paint exceed those of the traditional colorful stone-like paint. Moreover, the soft and hard details of the color points can achieve the expected effects only by adjusting the amount of borax used, and the formula design has a wider tolerance, is more convenient to operate, and has certain applicability. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:

[0054] Figure 1 The colorful stone-like paint prepared in Example 1 of the present invention;

[0055] Figure 2 This is a rendering of the colorful stone-like paint prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0056] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0057] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0058] The present invention will be described in detail below in conjunction with embodiments of the present invention, and each example is provided by way of explanation of the present invention without limiting the present invention. In fact, it will be clear to those skilled in the art that modifications and variations may be made in the present invention without departing from the scope or spirit of the present invention. For example, a feature shown or described as a part of an embodiment may be used in another embodiment to produce yet another embodiment. Therefore, it is desired that the present invention includes such modifications and variations within the scope of the appended claims and their equivalents.

[0059] In the embodiments and comparative examples of the present invention, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0060] The raw materials used in the examples and comparative examples of the present invention are shown in Table 1:

[0061] Table 1

[0062]

[0063]

[0064] Example 1

[0065] This embodiment provides a colorful stone-like paint, and the components and weight parts are shown in Table 2.

[0066] The preparation method of the colorful imitation stone coating of the present embodiment is as follows:

[0067] S1. Prepare borax solution: add borax and preservative into water in sequence, and stir evenly at a stirring rate of 500 r / min to obtain borax solution.

[0068] S2. Preparation of base paint, granulation liquid and continuous phase:

[0069] Base paint: add lithium magnesium silicate, dispersant, pigment filler, guar gum, defoamer, and multifunctional additive to water in sequence, adjust the speed of the disperser to 1500r / min, disperse for 30 minutes, adjust the speed to 500r / min, add polymer emulsion, antifreeze agent, film-forming aid, preservative, borax solution in sequence, adjust the speed to 1500r / min again, and finally add quartz sand and mix well to obtain base paint;

[0070] Granulating liquid: add lithium magnesium silicate, anti-settling agent, borax liquid and preservative into water in sequence, and stir evenly at a stirring rate of 500 r / min to obtain granulating liquid;

[0071] Continuous phase: add defoamer, multifunctional additive, antifreeze agent, film-forming additive, preservative, polymer emulsion and borax solution into water in sequence, and stir evenly at a stirring rate of 500r / min to obtain a continuous phase.

[0072] S3. Pour the prepared base paint and granulation liquid into a granulating agent, mix and granulate, and then add the continuous phase and mix evenly to obtain the colorful stone-like paint of this embodiment; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0073] Example 2

[0074] This embodiment provides a colorful stone-like paint, and the components and weight parts are shown in Table 2:

[0075] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 5:1:1.

[0076] Example 3

[0077] This embodiment provides a colorful stone-like paint, and the components and weight parts are shown in Table 2:

[0078] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 8:3:2.

[0079] Comparative Example 1

[0080] This comparative example provides a colorful stone-like paint, and the components and weight parts are shown in Table 2.

[0081] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0082] Comparative Example 2

[0083] This comparative example provides a colorful stone-like paint, and the components and weight parts are shown in Table 2.

[0084] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0085] Comparative Example 3

[0086] This comparative example provides a colorful stone-like paint, and the components and weight parts are shown in Table 2.

[0087] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0088] Comparative Example 4

[0089] This comparative example provides a colorful stone-like paint, and the remaining components and weight portions are the same as those in Example 1, except that the concentration of the borax solution in the base paint, granulation liquid and continuous phase in this comparative example is 0.5%.

[0090] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0091] Comparative Example 5

[0092] This comparative example provides a colorful stone-like paint, and the remaining components and weight portions are the same as those in Example 1, except that the concentration of the borax solution in the base paint, granulation liquid and continuous phase in this comparative example is 2.5%.

[0093] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0094] Comparative Example 6

[0095] This comparative example provides a colorful stone-like paint, and the components and weight portions are the same as those in Example 1.

[0096] The preparation method is the same as that of Example 1; the difference is that the mass ratio of the base paint, the granulation liquid and the continuous phase is 7:2:1.

[0097] Comparative Example 7

[0098] This comparative example provides a colorful stone-like paint, and the components and weight portions are the same as those in Example 1.

[0099] The preparation method is the same as that in Example 1; the difference is that the mass ratio of the base paint, the granulation liquid and the continuous phase is 4:2:1.

[0100] Comparative Example 8

[0101] This comparative example provides a colorful stone-like paint, and the components and weight parts are as follows:

[0102] Base paint: 25 parts water, 5 parts cellulose, 3 parts protective glue, 20 parts pigments and fillers, 25 parts polymer emulsion, 2 parts additives, 20 parts quartz sand

[0103] Granulation liquid: 60 parts of water, 3 parts of protective glue, 4 parts of compound, 3 parts of auxiliary agent, 30 parts of polymer latex.

[0104] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint to the granulation liquid is 5:1.

[0105] Comparative Example 9

[0106] This comparative example provides a colorful stone-like paint, and the remaining components and weight portions are the same as those in Example 1, except that 107 gum is used instead of guar gum.

[0107] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0108] Comparative Example 10

[0109] This comparative example provides a colorful stone-like paint, and the remaining components and weight portions are the same as those in Example 1, except that white latex is used instead of guar gum.

[0110] The preparation method is the same as that in Example 1; wherein the mass ratio of the base paint, the granulation liquid and the continuous phase is 6.5:2:1.5.

[0111] Table 2

[0112]

[0113]

[0114]

[0115]

[0116]

[0117] Test Example 1

[0118] The performance of the colorful imitation stone coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 8 was tested in indoor and outdoor environments, and the performance test items and standards were in accordance with HG / T4343-2012. The test results are shown in Tables 3 and 4:

[0119] Among them, water resistance determination methods include room temperature immersion method, boiling water immersion method, 40°C constant temperature flowing water immersion method, etc. The present invention adopts the room temperature immersion method. The national standard is GB / T 1733-1993. Prepare tools (1) Base plate: The base plate should be flat and without distortion, and the board surface should be free of any visible cracks and wrinkles. The size is 120mm*25mm*0.2-0.3mm test board; (2) distilled water or deionized water; (3) glass water tank. Then prepare the paint film on three test boards. Note that the test board should be sealed with a 1:1 mixture of paraffin and rosin before testing, and the sealing width is 2-3mm.

[0120] Room temperature immersion method

[0121] 1. Immersion of test panels

[0122] Add distilled or deionized water to the glass water tank. Adjust the water temperature to 23 +- 2 °C and maintain this temperature throughout the experiment.

[0123] Place three test panels in it and immerse 2 / 3 of the length of each test panel in water.

[0124] 2. Inspection of test panels

[0125] At the end of the immersion time specified in the product standard, take the test panel out of the tank, dry it with filter paper, and immediately or after conditioning it for the time specified in the product standard, visually inspect the test panel and record whether there is loss of gloss, discoloration, bubbles, wrinkles, shedding, rust, etc. and the recovery time.

[0126] At least two of the three test panels must meet the requirements of the product standards to be qualified.

[0127] Table 3 Technical requirements for water-based multi-color architectural coatings

[0128]

[0129]

[0130] Table 4 Performance technical requirements of water-based multi-color architectural coatings for exterior use

[0131]

[0132]

[0133]

[0134] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A colorful stone-like paint, characterized in that: The colorful stone-like paint comprises a base paint, a granulation liquid and a continuous phase; The base paint comprises the following components in parts by weight: 650-700 parts of water, 1-3 parts of lithium magnesium silicate, 55-65 parts of pigments and fillers, 2-3 parts guar gum, 150-250 parts of polymer emulsion, 750-850 parts of quartz sand, 1 to 3 parts of borax solution; 25-30 parts of additives; The granulation liquid comprises the following components in parts by weight: 750-800 parts of water, 4-6 parts of lithium magnesium silicate, 150-250 parts of borax solution, 2 to 4 parts of additives; The continuous phase comprises the following components in parts by weight: 250-300 parts of water, 550-650 parts of polymer emulsion, 40-60 parts of borax solution, 60-70 parts of additives.

2. The colorful stone-like paint according to claim 1, characterized in that: The mass ratio of the base paint, the granulation liquid and the continuous phase is (5-8):(1-3):(1-2).

3. The colorful stone-like paint according to claim 1, characterized in that: The borax liquid in the base paint, the borax liquid in the granulation liquid and the borax liquid in the continuous phase are all borax aqueous solutions; the mass concentration of borax in the borax aqueous solution is 1% to 2%.

4. The colorful stone-like paint according to claim 3, characterized in that: The borax aqueous solution also contains a preservative, the mass concentration of which is 1% to 2%; the preservative includes at least one of 1,2-benzisothiazolin-3-one, isothiazolinone and methylisothiazolinone.

5. The colorful stone-like paint according to any one of claims 1 to 4, characterized in that: The pigment and filler in the base paint includes at least one of titanium dioxide, kaolin and heavy calcium; And / or, the polymer emulsion in the base paint includes at least one of styrene acrylic emulsion, pure acrylic emulsion, and silicone acrylic emulsion; And / or, the additives in the base paint include the following components in parts by weight: 1-2 parts of dispersant, 1-2 parts of defoamer, 1-2 parts of multifunctional additive, 9-11 parts of antifreeze agent, 9-11 parts of film-forming additive, and 3-5 parts of preservative.

6. The colorful stone-like paint according to any one of claim 5, characterized in that: The auxiliary agent in the granulation liquid includes the following components in parts by weight: 1 to 2 parts of anti-settling agent, 1 to 3 parts of preservative; Preferably, the anti-settling agent comprises at least one of sodium carboxymethyl cellulose, a mixture of sodium carboxymethyl cellulose and xanthan gum in any proportion; the preservative comprises at least one of 1,2-benzisothiazolin-3-one, isothiazolinone and methylisothiazolinone; And / or, the auxiliary agent in the continuous phase includes the following components in parts by weight: 1-2 parts of defoaming agent, 1-2 parts of multifunctional auxiliary agent, 15-25 parts of antifreeze agent, 35-45 parts of film-forming auxiliary agent, and 1-3 parts of preservative; Preferably, the polymer emulsion in the continuous phase includes at least one of styrene acrylic emulsion, pure acrylic emulsion, and silicone acrylic emulsion.

7. The colorful stone-like paint according to claim 6, characterized in that: The dispersant in the base paint and the dispersant in the continuous phase are both at least one of anionic dispersants and non-ionic dispersants; the defoamer in the base paint and the defoamer in the continuous phase are both thick paste defoamers; the multifunctional additive in the base paint and the dispersant in the continuous phase are both 2-amino-2-methyl-1-propanol; the antifreeze in the base paint and the antifreeze in the continuous phase are both ethylene glycol; the film-forming aid in the base paint and the film-forming aid in the continuous phase are both alcohol ester dodecahydrate; the guar gum in the base paint is hydroxypropyl guar gum; the preservative in the base paint and the preservative in the continuous phase include at least one of 1,2-benzisothiazolin-3-one, isothiazolinone and methylisothiazolinone.

8. A method for preparing the colorful stone-like paint according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, prepare borax solution; S2, using the borax solution prepared in step S1 to prepare a base paint, a granulation liquid and a continuous phase respectively; S3, mixing the prepared basic paint and granulation liquid to form granules, and then adding the continuous phase to mix evenly to obtain the colorful stone-like paint.

9. The preparation method according to claim 8, characterized in that: In step S1, the process of preparing the borax solution specifically includes: adding borax and a preservative to water in sequence and stirring evenly to obtain the borax solution; And / or, in step S2, the process of preparing the base paint specifically comprises: adding lithium magnesium silicate, dispersant, pigment filler, guar gum, defoamer, and multifunctional additive to water in sequence, stirring at high speed and dispersing evenly, adding polymer emulsion, antifreeze agent, film-forming aid, preservative, and borax solution in sequence while continuing to slow down stirring, stirring at high speed again, and finally adding quartz sand and mixing evenly to obtain the base paint; And / or, in step S2, the process of preparing the granulation liquid specifically comprises: adding lithium magnesium silicate, an anti-settling agent, a borax solution, and a preservative into water in sequence and stirring the mixture to obtain the granulation liquid; And / or, in step S2, the process of preparing the continuous phase specifically includes: adding a defoaming agent, a multifunctional additive, an antifreeze agent, a film-forming aid, a preservative, a polymer emulsion, and a borax solution into water in sequence and stirring the mixture evenly to obtain the continuous phase.

10. The preparation method according to claim 9, characterized in that: In step S1, during the preparation of the borax solution, the stirring rate is 500-800 r / min; And / or, in step S2, during the process of preparing the base paint, the high-speed stirring rate is 1500-2000 r / min, the dispersion time is 30-40 min, and the reduced-speed stirring rate is 500-800 r / min; And / or, in step S2, during the process of preparing the granulation liquid, the stirring rate is 500-800 r / min; And / or, in step S2, during the process of preparing the continuous phase, the stirring rate is 500-800 r / min.

Citation Information

Patent Citations

  • Base paint of waterborne multicolor coating

    CN103319961A

  • Sand-in-sand multicolor paint and preparation method thereof

    CN113122099A

  • Lightweight and high-toughness sand-in-water multicolor paint and preparation method thereof

    CN115637080A

  • Preparation method of green low-carbon energy-saving light real stone paint

    CN116731572A

  • Base material of real stone paint as well as preparation method and application of base material

    CN117402530A

Cited By

  • Stone-like paint taking lithium magnesium silicate and guar gum as main bodies and introducing graphene family lamellar material as well as preparation method and application of stone-like paint

    CN121699452A