Preparation method of fluorinated ethylene propylene water-based paint with high hot melt adhesion

A high-heat-melt adhesive waterborne coating of perfluoroethylene propylene was prepared by emulsification treatment with polymer modifiers and inorganic fillers. This solved the problem of easy degumming of perfluoroethylene propylene coating at high temperature, improved the bonding strength and thermal stability of the coating, and met the requirements for high-temperature insulation.

CN118931273APending Publication Date: 2024-11-12WUXI SHUNXUAN NEW MATERIALS +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411271988.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Poly(fluoroethylene propylene) coatings are prone to delamination between the conductor and the coating during long-term high-temperature use, which affects the insulation and protection effect, and their heat resistance is not as good as that of polytetrafluoroethylene.

Method used

High-heat-melt adhesiveness polytetrafluoroethylene propylene waterborne coating was prepared by emulsifying polymer modifiers and inorganic fillers with FEP. The coating was obtained by processing with a vertical colloid mill and homogenizer, and then sprayed onto the surface of a PI film and baked at high temperature.

Benefits of technology

It improves the bonding strength and thermal stability between the coating and the metal conductor, reduces the difference in thermal expansion coefficients between the coating and the metal conductor, enhances the peel strength of the composite film, and meets the long-term protection requirements of high-temperature cable insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931273A_ABST
    Figure CN118931273A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a fluorinated ethylene propylene water-based coating with high hot melt adhesion, and belongs to the technical field of chemical materials. According to the invention, a polymer modifier and an inorganic filler are adopted as assistants, and are emulsified with FEP under the action of an emulsifier to obtain the high-hot-melt adhesive fluorinated ethylene propylene water-based paint. The obtained water-based paint can stably exist for a long time, and the coating appearance of the paint is smooth and compact. After high-temperature curing, the polymer modifier has good compatibility with FEP, and no phase separation condition is found microcosmically. The special molecular structure of the polymer modifier significantly improves the bonding strength and thermal stability of the FEP and the metal conductor, the inorganic filler improves the difference between the thermal expansion coefficients of the coating and the metal conductor, and the stripping force of the prepared composite film and metal is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical materials, and in particular relates to a method for preparing a high-thermal-melt-adhesive polyperfluoroethylene-propylene water-based coating. Background Art

[0002] Fluorinated ethylene propylene (FEP) is a copolymer of a small amount of perfluoropropyl perfluorovinyl ether and polytetrafluoroethylene, and is one of the modified varieties of polytetrafluoroethylene (PTFE). It has the advantages of excellent thermal stability, outstanding chemical inertness, good electrical insulation performance and low friction coefficient similar to PTFE. At the same time, thanks to the trifluoromethyl structure on the side chain, the melt adhesion of FEP is enhanced and the melt viscosity is reduced, which makes up for the difficulty of PTFE processing. FEP is often coated on the surface of PI film to play a role of hot melt bonding and is widely used in the surface insulation wrapping of high-temperature resistant wire and cable conductors. However, the heat resistance of FEP is not as good as PTFE. The upper temperature limit of F46 is 200℃, while the maximum operating temperature of polytetrafluoroethylene is 260℃. In long-term high-temperature use, the conductor and FEP coating are prone to debonding and peeling, affecting the insulation protection effect. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a high hot-melt adhesive polyperfluoroethylene propylene water-based coating, which is simple and easy to operate, and the obtained water-based coating can be stable for a long time, and the coating surface is smooth and dense.

[0004] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0005] A method for preparing a polyperfluoroethylene propylene water-based coating with high hot-melt adhesiveness comprises the following steps: using a polymer modifier and an inorganic filler as auxiliary agents, emulsifying them with FEP under the action of an emulsifier, and obtaining the polyperfluoroethylene propylene water-based coating with high hot-melt adhesiveness.

[0006] Furthermore, the polymer modifier is selected from one of polyphenylene sulfide powder, thermoplastic polyimide and polyether sulfone; the melt viscosity of the polyphenylene sulfide powder is 20-180 Pa.S; the melt viscosity of the thermoplastic polyimide is 20 Pa.S.

[0007] Furthermore, the usage ratio of the polymer modifier, the inorganic filler, the emulsifier and the FEP is 5-15:3:1.5:35-45.

[0008] Furthermore, the usage ratio of the polymer modifier, the inorganic filler, the emulsifier and the FEP is 15:3:1.5:35.

[0009] Furthermore, the inorganic filler is chromium trioxide.

[0010] Furthermore, the emulsifier is propylene glycol diacetate.

[0011] Furthermore, the preparation method of any of the above-mentioned high hot-melt adhesive polyperfluoroethylene-propylene water-based coatings comprises the following steps:

[0012] (1) By weight, 5 to 15 parts of polyphenylene sulfide powder, 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly and ground using a vertical colloid mill for 60 minutes;

[0013] (2) Add 35-45 parts of FEP powder and 1.5 parts of propylene glycol diacetate to the ground mixed solution, and emulsify it with a homogenizer to obtain a high hot-melt adhesive polyperfluoroethylene propylene water-based coating.

[0014] Furthermore, in the step (2), the speed of the homogenizer is 10000 rpm and the emulsification time is 30 min.

[0015] Furthermore, the high hot melt adhesive polyperfluoroethylene propylene water-based coating is prepared by any of the above methods.

[0016] Furthermore, the coating was directly sprayed on the surface of the PI film and baked at 390° C. for 10 min to obtain a fluorinated polyimide film.

[0017] Compared with the prior art, the advantages of the present invention are as follows:

[0018] 1) The water-based coating prepared by the present invention can exist stably for a long time, and the coating surface is smooth and dense.

[0019] 2) After high temperature curing, the polymer modifier of the present invention has good compatibility with FEP, and no phase separation is found at the microscopic level.

[0020] 3) The present invention adopts the special molecular structure of the polymer modifier to significantly improve the bonding strength and thermal stability between FEP and the metal conductor, and the inorganic filler improves the difference in thermal expansion coefficient between the coating and the metal conductor, and the peeling force between the prepared composite film and the metal is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a scanning electron microscope image of the coating obtained in Example 3 of the present invention after curing;

[0022] Figure 2 This is a scanning electron microscope image of the coating of Comparative Example 2 after curing;

[0023] Figure 3 It is a comparison chart of peeling force test curves of various embodiments and comparative examples. DETAILED DESCRIPTION

[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0025] Unless otherwise specified, the raw materials or reagents used in the following examples are commercially available products or products prepared by conventional methods in the laboratory.

[0026] Example 1

[0027] A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, the steps are as follows:

[0028] By weight, 15 parts of polyphenylene sulfide powder (melt viscosity 180 Pa.S), 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly and ground for 60 minutes using a vertical colloid mill; 35 parts of FEP powder and 1.5 parts of propylene glycol diacetate were added to the ground mixture, and emulsified at 10000 rpm for 30 minutes using a homogenizer to obtain a high hot melt adhesive polyperfluoroethylene propylene water-based coating.

[0029] Example 2

[0030] A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, the steps are as follows:

[0031] By weight, 15 parts of polyphenylene sulfide powder (melt viscosity 100 Pa.S), 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly and ground for 60 minutes using a vertical colloid mill; 35 parts of FEP powder and 1.5 parts of propylene glycol diacetate were added to the ground mixture, and emulsified at 10000 rpm by a homogenizer for 30 minutes to obtain a high hot-melt adhesive polyperfluoroethylene propylene water-based coating.

[0032] Example 3

[0033] A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, the steps are as follows:

[0034] By weight, 15 parts of polyphenylene sulfide powder (melt viscosity 20 Pa.S), 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly, and ground for 60 minutes using a vertical colloid mill; then 35 parts of FEP powder and 1.5 parts of propylene glycol diacetate were added to the ground mixture, and emulsified at 10000 rpm for 30 minutes using a homogenizer to obtain a high hot melt adhesive polyperfluoroethylene propylene water-based coating.

[0035] Example 4

[0036] A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, the steps are as follows:

[0037] By weight, 5 parts of polyphenylene sulfide powder (melt viscosity 20 Pa.S), 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly, and ground for 60 minutes using a vertical colloid mill; then 45 parts of FEP powder and 1.5 parts of propylene glycol diacetate were added to the ground mixture, and emulsified at 10000 rpm by a homogenizer for 30 minutes to obtain a high hot-melt adhesive polyperfluoroethylene propylene water-based coating.

[0038] Example 5

[0039] A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, the steps are as follows:

[0040] By weight, 15 parts of thermoplastic polyimide (melt viscosity 20 Pa.S), 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly, and ground for 60 minutes using a vertical colloid mill; then 35 parts of FEP micropowder and 1.5 parts of propylene glycol diacetate were added to the ground mixture, and emulsified at 10000 rpm for 30 minutes using a homogenizer to obtain a high hot melt adhesive polyperfluoroethylene propylene water-based coating.

[0041] Example 6

[0042] A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, the steps are as follows:

[0043] By weight, 15 parts of polyethersulfone, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly and ground for 60 minutes using a vertical colloid mill; 35 parts of FEP micropowder and 1.5 parts of propylene glycol diacetate were added to the ground mixture, and emulsified at 10,000 rpm with a homogenizer for 30 minutes to obtain a high hot-melt adhesive polyperfluoroethylene propylene water-based coating.

[0044] Comparative Example 1

[0045] A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, the steps are as follows:

[0046] By weight, 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly and ground for 60 minutes using a vertical colloid mill; 35 parts of FEP micropowder and 1.5 parts of propylene glycol diacetate were added to the ground mixture, and emulsified at 10,000 rpm with a homogenizer for 30 minutes to obtain a high hot-melt adhesive polyperfluoroethylene propylene water-based coating.

[0047] Comparative Example 2

[0048] A commercially available FEP concentrated dispersion was directly sprayed on the surface of the PI film (coating thickness 12 μm) and then baked at high temperature to form the film.

[0049] The coatings prepared in the above-mentioned embodiments and comparative examples were sprayed on the surface of the PI film (coating thickness: 12 μm), and baked at 390° C. for 10 min to obtain a fluorinated polyimide film.

[0050] The morphology of the coating was observed using scanning electron microscopy. Figure 1 As shown, Figure 1 is a scanning electron microscope image of the coating after curing in Example 3; Figure 2 As shown, Figure 2 This is a scanning electron microscope image of the coating of Comparative Example 2 after curing.

[0051] Depend on Figure 1 and Figure 2 It can be seen that a large number of microcracks exist on the surface of the commercial FEP emulsion coating after curing, while the coating of the present invention is more compact at the microscopic level and has no obvious phase separation, which proves that the polymer modifier has good compatibility with the FEP resin.

[0052] like Figure 3 As shown, the peeling force between the coated PI film and the copper sheet was tested after hot pressing at 380℃ and 20psi. The hot pressed samples were placed in a high and low temperature cycle test box, with a low temperature of 25℃ and a high temperature of 250℃. The peeling force was measured again after 100 cycles. The test results are shown in Table 1 below.

[0053] Table 1 Comparison of peeling strength between PI film with coating and copper sheet prepared in Examples 1 to 6 and Comparative Examples 1 to 2

[0054]

[0055]

[0056] It can be seen from the data in Table 1 that when the melt viscosity of the polymer modifier is in an appropriate range, the modified coating has good film-forming properties at high temperatures and its peeling force is significantly better than that of pure commercial FEP concentrated dispersion.

[0057] The maximum peeling force of Example 3 is 2.2 times that of the commercial FEP concentrated dispersion, and the average peeling force is also increased by 2.8 times. This is mainly because the polymer modifier forms a network structure chelate with the metal surface particles at high temperature, which significantly improves the adhesion between the FEP coating and the metal. After the inorganic filler is filled, the difference in thermal expansion coefficient between the coating and the metal is reduced, and there is no phase separation after curing. After the composite film undergoes high and low temperature cycles, the peeling force does not significantly decay, which can meet the long-term protection requirements of high temperature resistant cable insulation.

[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high hot melt adhesive polyperfluoroethylene propylene water-based coating, characterized in that: A high molecular modifier and an inorganic filler are used as auxiliary agents, which are emulsified with FEP under the action of an emulsifier to obtain a high hot-melt adhesive polyperfluoroethylene-propylene water-based coating.

2. The method for preparing the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to claim 1, characterized in that: The polymer modifier is selected from one of polyphenylene sulfide powder, thermoplastic polyimide and polyether sulfone; the polyphenylene sulfide powder has a melt viscosity of 20 to 180 Pa.S; the thermoplastic polyimide has a melt viscosity of 20 Pa.S.

3. The method for preparing the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to claim 1, characterized in that: The usage ratio of the polymer modifier, the inorganic filler, the emulsifier and the FEP is 5-15:3:1.5:35-45.

4. The method for preparing the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to claim 3, characterized in that: The usage ratio of the polymer modifier, the inorganic filler, the emulsifier and the FEP is 15:3:1.5:

35.

5. The method for preparing the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to claim 1, characterized in that: The inorganic filler is chromium trioxide.

6. The method for preparing the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to claim 1, characterized in that: The emulsifier is propylene glycol diacetate.

7. The method for preparing the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to any one of claims 1 to 6, characterized in that: Here are the steps: (1) By weight, 5 to 15 parts of polyphenylene sulfide powder, 3 parts of chromium trioxide, 1.5 parts of perfluorooctanoic acid and 44 parts of water were mixed evenly and ground using a vertical colloid mill for 60 minutes; (2) Add 35-45 parts of FEP powder and 1.5 parts of propylene glycol diacetate to the ground mixed solution, and emulsify it with a homogenizer to obtain a high hot-melt adhesive polyperfluoroethylene propylene water-based coating.

8. The method for preparing the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to claim 7, characterized in that: In the step (2), the speed of the homogenizer is 10000 rpm and the emulsification time is 30 min.

9. A water-based polyperfluoroethylene propylene coating with high hot melt adhesiveness prepared according to the method of any one of claims 1 to 8.

10. The use of the high hot melt adhesive polyperfluoroethylene propylene water-based coating according to claim 9 in the preparation of fluorinated polyimide film, characterized in that: The coating was directly sprayed on the surface of the PI film and baked at 390°C for 10 minutes to obtain a fluorinated polyimide film.

Citation Information

Patent Citations

  • Emulsion for polyimide film fluorine-containing coating

    CN103897514A

  • Process of applying a fluoropolymeric coating to a polyimide film

    GB1126012A