High-performance environment-friendly water-based paint as well as preparation method and application thereof

By adding bentonite, alumina powders and crosslinking agents of specific particle sizes to the aqueous resin, the problem of insufficient coating hardness and weather resistance of existing water-based automotive coatings is solved, and the low VOC of high-performance environmentally friendly water-based coatings is achieved Emissions and excellent decorative properties have promoted the green transformation of the coatings industry.

CN118931283AActive Publication Date: 2024-11-12QINGYUAN HUAYUAN INST OF SCI & TECH COLLABORATIVE INNOVATION CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411171716.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing water-based automotive coatings have shortcomings in preparation technology and coating performance, such as low coating hardness, poor weather resistance, and difficult construction, which is difficult to meet the needs of environmental protection and high performance.

Method used

Use aqueous resin as the film-forming substrate, add bentonite and alumina powder of specific particle sizes, add crosslinking agents and functional additives to enhance mechanical properties and weather resistance through small size and surface effects of nanoparticles, and chemically The reaction forms a tight three-dimensional mesh structure, which improves the hardness and scratch resistance of the paint.

Benefits of technology

It has achieved low VOC emissions, high weather resistance, strong scratch resistance and excellent decorative properties of high-performance environmentally friendly water-based coatings, providing green and efficient solutions for the automotive coating industry, and promoting the green transformation and ability of the coating industry. Continuous development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005009469190000041
    Figure BDA0005009469190000041
  • Figure BDA0005009469190000051
    Figure BDA0005009469190000051
  • Figure BDA0005009469190000052
    Figure BDA0005009469190000052
Patent Text Reader

Abstract

The invention discloses a high-performance environment-friendly water-based coating as well as a preparation method and application thereof, and relates to the technical field of coatings. The high-performance environment-friendly water-based paint comprises the following components in parts by mass: 59-74 parts of water-based resin; 10 to 20 parts of powder; 0.1 to 0.5 part of a cross-linking agent; 0.5 to 0.9 part of a functional auxiliary agent; 15 to 20 parts of a solvent; the powder comprises bentonite and aluminum oxide, the D50 particle size of the bentonite is 25-30 nm, and the D50 particle size of the aluminum oxide is 10-15 nm. The water-based paint disclosed by the invention has excellent weather resistance, scratch resistance and mechanical properties, and is beneficial to low VOC (Volatile Organic Compound) emission, high weather resistance, strong scratch resistance and excellent decorative property of the paint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and in particular to a high-performance, environment-friendly water-based coating and a preparation method and application thereof. Background Art

[0002] With the increasing global awareness of environmental protection and increasingly stringent environmental regulations, the automotive coatings industry is gradually shifting from solvent-based to water-based. However, the current water-based automotive coatings on the market still have many deficiencies in terms of preparation process and coating performance, such as low coating hardness, poor weather resistance, and difficulty in construction.

[0003] Therefore, it is of great significance to develop a high-performance, environmentally friendly water-based coating. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a high-performance environmentally friendly water-based paint and its preparation method and application. The water-based paint of the present invention has excellent weather resistance, scratch resistance and mechanical properties, is conducive to low VOC emissions, high weather resistance, strong scratch resistance and excellent decorative properties of the paint, and provides a green and efficient solution for the automotive coating industry.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] In a first aspect, the present invention provides a high-performance environmentally friendly water-based coating, comprising the following components in parts by weight:

[0007] 59-74 parts of water-based resin; 10-20 parts of powder; 0.1-0.5 parts of cross-linking agent; 0.5-0.9 parts of functional additives; 15-20 parts of solvent;

[0008] The powder comprises bentonite and alumina, wherein the D50 particle size of the bentonite is 25-30 nm, and the D50 particle size of the alumina is 10-15 nm.

[0009] The present invention adopts water-based resin as the film-forming substrate of coating, and by adding powder, utilizing the small size effect and surface effect of nanoparticles, it is beneficial to enhance the mechanical properties and weather resistance of coating, and by compounding bentonite and alumina of specific particle size, the hardness, wear resistance and scratch resistance of coating can be further enhanced. By adding a cross-linking agent, it is beneficial to improve the scratch resistance and adhesion of coating, and ensure the stability and durability of coating under complex environment. By adding functional additives, the processing performance and coating quality of coating can be improved. Therefore, the present invention is beneficial to improve the weather resistance, scratch resistance and mechanical properties of coating by adding powder, cross-linking agent and functional additives in water-based resin.

[0010] Preferably, the cross-linking agent comprises hexamethoxymethylolmelamine and butylated melamine.

[0011] Preferably, the mass ratio of hexamethoxymethylolmelamine to butylated melamine is 1:(2-5).

[0012] The invention adopts hexamethoxymethylol melamine and butylated melamine as crosslinking agents, which can form a compact and stable three-dimensional (stereoscopic) network structure through chemical reaction crosslinking with water-based resin, which is beneficial to improve the hardness, scratch resistance, weather resistance and wear resistance of the coating.

[0013] Preferably, the high-performance environmentally friendly water-based coating comprises the following components in parts by weight:

[0014] 60-70 parts of water-based resin; 12-15 parts of powder; 0.2-0.4 parts of cross-linking agent; 0.6-0.8 parts of functional additives; 17-19 parts of solvent.

[0015] Preferably, the water-based resin includes water-based acrylic resin or polyurethane resin.

[0016] Preferably, the solvent is water.

[0017] The present invention adopts water as a solvent, VOC emission is extremely low, and the coating meets environmental protection requirements.

[0018] Preferably, the functional additive includes at least one of a thickener, a dispersant, a defoaming agent, and a film-forming aid.

[0019] More preferably, the thickener includes a cellulose thickener or a polyacrylic acid thickener; the dispersant includes dispersant TENLO70 or dispersant SDJ8005; the defoaming agent includes polydimethylsiloxane; and the film-forming aid includes at least one of Texanol alcohol ester, Coasol, and Nexcoat795.

[0020] In a second aspect, the present invention also provides a method for preparing a high-performance environmentally friendly water-based coating, comprising the following steps:

[0021] (1) mixing the powder with the water-based resin, half of the solvent and the functional additive to obtain a pre-dispersion liquid;

[0022] (2) The pre-dispersed liquid is mixed evenly with the other half of the solvent and the cross-linking agent to obtain a high-performance, environmentally friendly water-based coating.

[0023] In a third aspect, the present invention also provides a high-performance, environmentally friendly water-based paint for use in automobiles.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The high-performance, environmentally friendly water-based paint described in the present invention can not only meet the demand of the automotive coating industry for environmentally friendly, high-performance coatings, but also promote the green transformation and sustainable development of the coating industry, and gradually replace traditional solvent-based coatings to become a mainstream product in the automotive coating market. DETAILED DESCRIPTION

[0026] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the protection scope and implementation methods of the present invention are not limited thereto.

[0027] Unless otherwise specified, the materials and reagents used in the following examples are commercially available.

[0028] Examples 1-11

[0029] The embodiments of the high-performance environmentally friendly water-based paint and the preparation method thereof of the present invention, the components of the high-performance environmentally friendly water-based paint are shown in Table 1.

[0030] The method for preparing the high-performance environmentally friendly water-based coating comprises the following steps:

[0031] (1) Put the powder into a container, then add a dispersant, half of the defoamer and half of the solvent, disperse it in a high-speed stirrer for 10 minutes, and shake it in a high-speed shaker for 1 hour to obtain a pre-dispersion liquid;

[0032] (2) adding the pre-dispersed liquid to the aqueous resin, then adding the thickener, the film-forming aid and the remaining half of the defoamer, mixing, and dispersing for another 30 minutes with a high-speed stirrer to obtain a nanocomposite emulsion;

[0033] (3) Add the cross-linking agent to the nano-composite emulsion in a mass ratio of 0.5:1, stir and mix at 30°C, and add the remaining half of the solvent at any time to adjust the viscosity to 25S, thereby obtaining a high-performance environmentally friendly water-based coating.

[0034] Comparative Examples 1-6

[0035] The difference between each comparative example and the embodiment is only in the type and proportion of components, as shown in Table 2.

[0036] Among the components described in each embodiment and comparative example:

[0037] The water-based resin 1 is a water-based acrylic resin, model LB-1015, Shenzhen Lanbo Environmental Protection Technology Co., Ltd.;

[0038] The water-based resin 2 is a polyurethane resin, model LB-80, from Shenzhen Lanbo Environmental Protection Technology Co., Ltd.

[0039] The powder 1 includes bentonite and alumina, wherein the D50 particle size of the bentonite is 25 nm, and the D50 particle size of the alumina is 10 nm;

[0040] The powder 2 includes bentonite and alumina, wherein the D50 particle size of the bentonite is 25 nm, and the D50 particle size of the alumina is 15 nm;

[0041] The powder 3 includes bentonite and alumina, wherein the D50 particle size of the bentonite is 30 nm, and the D50 particle size of the alumina is 10 nm;

[0042] The powder 4 includes bentonite and alumina, wherein the D50 particle size of the bentonite is 30 nm, and the D50 particle size of the alumina is 15 nm;

[0043] The powder 5 includes bentonite and alumina, wherein the D50 particle size of the bentonite is 15 nm, and the D50 particle size of the alumina is 10 nm;

[0044] The powder 6 includes bentonite and alumina, wherein the D50 particle size of the bentonite is 25 nm, and the D50 particle size of the alumina is 25 nm;

[0045] The powder 7 includes bentonite;

[0046] The powder 8 includes aluminum oxide;

[0047] The powder 9 includes bentonite and silicon dioxide;

[0048] The powder 10 includes silicon dioxide and aluminum oxide.

[0049] The cross-linking agent 1 is hexamethoxymethylol melamine;

[0050] The cross-linking agent 2 comprises hexamethoxymethylol melamine and butylated melamine, and the mass ratio of hexamethoxymethylol melamine to butylated melamine is 1:2;

[0051] The cross-linking agent 3 comprises hexamethoxymethylol melamine and butylated melamine, and the mass ratio of hexamethoxymethylol melamine to butylated melamine is 1:3;

[0052] The cross-linking agent 4 comprises hexamethoxymethylol melamine and butylated melamine, and the mass ratio of hexamethoxymethylol melamine to butylated melamine is 1:4;

[0053] The cross-linking agent 5 includes hexamethoxymethylol melamine and butylated melamine, and the mass ratio of hexamethoxymethylol melamine to butylated melamine is 1:5.

[0054] The functional additives include a thickener, a dispersant, a defoamer, and a film-forming aid, and the mass ratio of the four is 1:1:1:1;

[0055] The thickener is hydroxyethyl cellulose, model 250HBR, Mairui New Materials; the dispersant is dispersant SDJ8005, Guangdong Dingjia New Materials Technology Co., Ltd.; the defoaming agent is polydimethylsiloxane, Foshan Guirunbao Biotechnology Co., Ltd.; and the film-forming aid is Texanol alcohol ester, Eastman.

[0056] The solvent is deionized water.

[0057] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.

[0058] Table 1

[0059]

[0060]

[0061] Table 2

[0062]

[0063]

[0064] In order to verify the performance of the high-performance environmentally friendly water-based coating of the present invention, the high-performance environmentally friendly water-based coating prepared in each embodiment and comparative example was sprayed on tinplate with a coating thickness of 25±um and baked at 60°C for 30 minutes to obtain a pre-coated plate sample for performance evaluation test.

[0065] Performance testing method:

[0066] 1. Gloss: Tested in accordance with GB / T9754-2007 standard.

[0067] 2. Hardness: Tested in accordance with GB / T6739-2006 standard. The higher the hardness grade, the greater the hardness.

[0068] 3. Adhesion: Tested according to GB / T9286-1998 standard. The lower the adhesion grade, the better the adhesion.

[0069] 4. Scratch resistance: measured by Nano Indenter XP (MTS Inc., USA), load 1 mN.

[0070] 5. Salt spray resistance: tested in accordance with ISO9227-2012 standard.

[0071] 6. VOC: Tested in accordance with GB / T23985-2009 standard.

[0072] 7. Abrasion resistance: The surface of the coating was polished with RCA paper tape, produced by Norman Tool Company.

[0073] The performance parameters obtained from the above tests are shown in Tables 3 and 4.

[0074] Table 3

[0075]

[0076] Table 4

[0077]

[0078]

[0079] According to Table 3, the glossiness of the high-performance environmentally friendly water-based paint of the present invention is greater than 92%, indicating that the paint has a good decorative effect; and the hardness grade of the paint is above 2H, the adhesion grade is 0, the scratch resistance can reach 8.42-9.81GPa, and the wear resistance can reach more than 1200 times, indicating that the high-performance environmentally friendly water-based paint of the present invention has excellent hardness, adhesion, scratch resistance, wear resistance and weather resistance.

[0080] According to the comparison between Comparative Examples 1-6 and Example 2, it can be obtained that in Comparative Examples 3-4, bentonite or alumina is used as powder alone, and the hardness, scratch resistance and wear resistance of the coating are not as good as those in Example 2, while in Example 2, bentonite and alumina are compounded, which can not only enhance the hardness, wear resistance and scratch resistance of the coating, but also improve the adhesion and weather resistance of the coating. In Comparative Examples 5-6, bentonite or alumina is compounded with silicon dioxide, and the weather resistance, scratch resistance and wear resistance of the coating are all lower than those in Example 2, indicating that the effect of the present invention can not be achieved by compounding with any powder in the present invention. The particle size of bentonite or alumina in Comparative Examples 1-2 is not within the range defined by the present invention, and the adhesion, scratch resistance and wear resistance of the coating are all lower than those in Example 2, indicating that in the present invention, only by compounding bentonite and alumina with specific particle sizes can the coating have excellent weather resistance, scratch resistance, decorativeness and wear resistance at the same time.

[0081] According to the comparison between Examples 6-9 and Example 2, the crosslinking agent in Example 2 is hexamethoxymethylol melamine, and the crosslinking agent in Example 6 is compounded with hexamethoxymethylol melamine and butylated melamine. The hardness, scratch resistance and wear resistance of the coating are all greater than those of Example 2, indicating that compounding hexamethoxymethylol melamine and butylated melamine is beneficial to improving the weather resistance, scratch resistance and wear resistance of the coating. The mass ratio of hexamethoxymethylol melamine and butylated melamine in Examples 6-9 gradually increases, and the gloss and scratch resistance of the coating first increase and then decrease, indicating that the present invention can achieve the best performance of the coating by controlling the mass ratio of hexamethoxymethylol melamine and butylated melamine to 1: (2-5).

[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A high-performance environmentally friendly water-based paint, characterized in that: The composition comprises the following components in parts by weight: 59-74 parts of water-based resin; 10-20 parts of powder; 0.1-0.5 parts of cross-linking agent; 0.5-0.9 parts of functional additives; 15-20 parts of solvent; The powder comprises bentonite and alumina, wherein the D50 particle size of the bentonite is 25-30 nm, and the D50 particle size of the alumina is 10-15 nm.

2. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The crosslinking agent includes hexamethoxymethylolmelamine and butylated melamine.

3. The high performance environmentally friendly water-based paint according to claim 2, characterized in that: The mass ratio of the hexamethoxymethylolmelamine to butylated melamine is 1:(2-5).

4. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The water-based resin includes water-based acrylic resin or polyurethane resin.

5. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The solvent is water.

6. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The functional additive includes at least one of a thickener, a dispersant, a defoamer, and a film-forming aid.

7. The high performance environmentally friendly water-based paint according to claim 6, characterized in that: The thickener includes a cellulose thickener or a polyacrylic acid thickener; and the defoaming agent includes polydimethylsiloxane.

8. The high performance environmentally friendly water-based paint according to claim 6, characterized in that: The film-forming aid includes at least one of Texanol alcohol ester, Coasol, and Nexcoat795.

9. The method for preparing a high-performance, environmentally friendly water-based coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) mixing the powder with the water-based resin, half of the solvent and the functional additive to obtain a pre-dispersion liquid; (2) The pre-dispersed liquid is mixed evenly with the other half of the solvent and the cross-linking agent to obtain a high-performance, environmentally friendly water-based coating.

10. Use of the high-performance, environmentally friendly water-based paint according to any one of claims 1 to 8 in automobiles.

Citation Information

Patent Citations

  • Water-based high-performance stoving varnish

    CN109627932A

  • High-performance waterborne automobile varnish and preparation method thereof

    CN110564242A

  • Water-based single-component wood coating and preparation method thereof

    CN111171691A

  • Scrape-wearable nanometer aqueous automobile paint preparation method

    CN1970663A

  • Water-soluble inoganic hard coating composition for protecting of metal surface

    KR101201756B1