Anti-warping core layer and preparation method thereof

By using the anti-warping core layer technology in high-performance optical films, the warping problem caused by uneven expansion coefficient is solved, the thermal stability and anti-aging properties of the film are improved, and the service life is extended, and the solution is achieved The goal of warping does not affect the membrane performance.

CN118931310APending Publication Date: 2024-11-12湖南壹鑫科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027873.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the production process, traditional high-performance optical films cause warping due to uneven expansion coefficients, which affects service life. The existing methods also affect the performance of the film when solving warping.

Method used

Using an anti-warping core layer, including epoxy resin, curing agent, ionic gel, modified beeswax, anti-compression hardener, filler and diluent, through specific formula ratios and preparation methods, good thermal stability is formed. and anti-aging anti-warping layer to avoid warping caused by temperature changes.

Benefits of technology

The warping resistance and stability of the high-performance optical film is improved, and the service life is extended, achieving the goal of not affecting the film performance while solving warping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931310A_ABST
    Figure CN118931310A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high-performance coating materials, and discloses an anti-warping core layer and a preparation method thereof.The anti-warping core layer is prepared by coating a base film with a prepared anti-warping solution, the anti-warping solution comprises the following components in parts by weight: 15-25 parts of epoxy resin, 4-10 parts of a curing agent, 5-10 parts of ionic gel, 5-10 parts of silicic acid gel, 0.5-3 parts of modified beewax, 0.5-5 parts of filler, 0.5-1 part of a compression-resistant hardening agent and 55-65 parts of a diluent. The modified beeswax and the compression-resistant hardening agent added into the anti-warping core layer have good thermal stability and aging resistance, so that the internal structure of the core layer is uniform and stable, warping caused by mismatching of thermal expansion coefficients is avoided, and the performance stability can be continuously kept in the life cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-performance coating materials, and more specifically discloses an anti-warping core layer and a preparation method thereof. Background Art

[0002] With the continuous development of high-performance optical film technology, high-performance optical films are widely used in liquid crystal display, car beauty, mobile phone protection, photovoltaic and other fields, and the requirements for high-performance optical films are constantly increasing. However, due to the uneven expansion coefficient during the production process, traditional high-performance optical films will cause the film to warp due to temperature changes, which seriously affects the service life of the film. To solve the warping problem, the common method in the industry is to add a large amount of low-shrinkage additives (such as polyvinyl acetate, polymethyl methacrylate, polystyrene) to the coating to reduce the shrinkage of the coating or film to a certain extent. Although these methods can appropriately solve the warping problem, the corresponding service life of these high-performance optical films is also affected to a certain extent. Summary of the invention

[0003] The purpose of the present invention is to provide a warping-resistant core layer and a preparation method thereof, so as to solve the problem that the service life of the high-performance optical film is also affected to a certain extent while solving the warping problem in the current method.

[0004] To solve the above technical problems, according to one aspect of the present invention, more specifically, an anti-warping core layer comprises a substrate layer coated with a formulated anti-warping solution, the anti-warping solution comprising the following components: epoxy resin, curing agent, ion gel, silica gel, modified beeswax, compressive hardener, filler, and diluent.

[0005] The added compressive hardener makes the core layer have good thermal stability and aging resistance, thereby preventing the finished film from warping due to temperature changes. The modified beeswax can accelerate nucleation and promote the coagulation of the anti-warping solution.

[0006] Furthermore, the anti-warping solution includes the following components by weight: 15 to 25 parts of epoxy resin, 4 to 10 parts of curing agent, 5 to 10 parts of ion gel, 5 to 10 parts of silica gel, 0.5 to 3 parts of modified beeswax, 0.5 to 5 parts of filler, 0.5 to 1 part of anti-compression hardener, and 55 to 65 parts of diluent.

[0007] Furthermore, the epoxy resin of the present invention includes at least one of hydrogenated bisphenol A diglycidyl ether, phenol-type novolac epoxy resin, and o-cresol-type novolac epoxy resin;

[0008] Furthermore, the curing agent of the present invention includes at least one of polyvinyl ester resin, polyacrylic acid resin, and organosilicon-modified polyacrylic acid resin;

[0009] Furthermore, the ion gel of the present invention is obtained by polymerizing an imidazole cationic liquid monomer and an acid radical or imide anionic liquid monomer, wherein the imidazole cationic liquid monomer is at least one of 1-aminopropyl-3-methylimidazolium cation, 1-aminoethyl-3-methylimidazolium cation, 1-vinyl-3-methylimidazolium cation, and 1-decyl-3-methylimidazolium cation; the acid radical or imide anionic liquid monomer is at least one of tetrafluoroborate anion, hexafluorophosphate anion, and bistrifluoromethanesulfonyl imide anion;

[0010] Furthermore, the silica gel of the present invention includes at least one of 3% sodium silicate gel, 5% sodium silicate gel, and 7% sodium silicate;

[0011] Furthermore, the modified beeswax in the present invention includes at least one of modified Chinese beeswax and modified Western beeswax;

[0012] Furthermore, the compressive hardening agent of the present invention is a potassium tantalate ternary complex, which is prepared by suspending potassium carbonate powder in catechol, adding oxalic acid to adjust the pH to 1 under stirring, and stirring at room temperature for 4 hours;

[0013] Furthermore, the filler of the present invention includes any one of white carbon black, glass fiber, and precipitated barium sulfate;

[0014] Furthermore, the diluent of the present invention includes any one of resorcinol diglycidyl ether, β-hydroxyethyl methacrylate, 1,6-hexanediol diacrylate, and polypropylene glycol diglycidyl ether.

[0015] According to another aspect of the present invention, there is provided a method for preparing an anti-warping core layer, comprising the following steps:

[0016] S1, adding the formulated amount of epoxy resin into the diluent, stirring to dissolve, and recording as the first mixed system;

[0017] S2, add cations to water, add anions in batches under stirring, adjust pH by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add the formulated amount of ion gel and silica gel to the first mixed system obtained in step S1, stir and dissolve, and record it as the second mixed system;

[0018] S3, adding beeswax to a diluent, heating to melt, dropping a sodium carbonate solution, adjusting the pH, and cooling to obtain a modified beeswax; adding a formula amount of modified beeswax and a filler to the second mixed system obtained in step S2, stirring to dissolve, and recording as a third mixed system;

[0019] S4, adding the formulated amount of curing agent to the diluent, stirring and dissolving, and recording as the fourth mixing system;

[0020] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0021] S6, suspending potassium carbonate powder in catechol, adding oxalic acid to adjust pH≈1 under stirring, stirring at room temperature for 4 hours, filtering, and adding the filtrate to the fifth mixed system obtained in step S5, stirring and mixing, and recording as the sixth mixed system

[0022] S7. Prepare a base film, apply the sixth mixed system on the upper surface of the substrate layer by atomizing spraying, ultrasonic spraying, or anilox roller coating, and then age it under ultraviolet light to obtain an anti-warping core layer with a thickness of 150 to 210 μm.

[0023] Beneficial Effects

[0024] The present invention discloses an anti-warping core layer and a preparation method thereof, which provides an effective anti-warping layer for high-performance optical films and is used in the fields of liquid crystal display, car beauty, mobile phone protection, photovoltaics, etc. The anti-warping layer has good thermal stability and aging resistance, so that it can improve the anti-warping ability and stability of high-performance optical films and increase their service life.

[0025] The anti-warping core layer of the present invention can be used as a finished high-performance optical film to provide anti-warping performance according to needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the structure of the potassium tantalate ternary complex of the present invention. DETAILED DESCRIPTION

[0027] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.

[0028] Embodiment 1

[0029] S1, adding 15 parts of o-cresol type novolac epoxy resin to 45 parts of resorcinol bisglycidyl ether, stirring to dissolve, recorded as the first mixed system;

[0030] S2, add 1-aminoethyl-3-methylimidazolium cation to water, add hexafluorophosphate anion in batches under stirring, adjust the pH to 6-7 by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add 5 parts of the prepared ion gel and 5 parts of 5% sodium silicate gel to the first mixed system obtained in step S1, stir and dissolve, and record as the second mixed system;

[0031] S3, adding beeswax to a diluent, heating to melt, dropping 2M sodium carbonate solution, adjusting the pH to 7-8, and cooling to obtain modified beeswax; adding 0.5 parts of modified beeswax and 0.5 parts of glass fiber to the second mixed system obtained in step S2, stirring to dissolve, and recording as the third mixed system;

[0032] S4, adding 7 parts of organosilicon-modified polyacrylic acid resin to 10 parts of resorcinol bisglycidyl ether, stirring to dissolve, and recording as the fourth mixing system;

[0033] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0034] S6, suspend 0.5 parts of potassium carbonate powder in catechol, add oxalic acid to adjust pH≈1 under stirring, stir at room temperature for 4 hours, filter, add the filtrate to the fifth mixed system obtained in step S5, stir and mix, and record it as the sixth mixed system

[0035] S7. The sixth mixed system is coated on the surface of the PET base film by atomizing spraying, and then aged under ultraviolet light to obtain an anti-warping core layer with a thickness of 150 μm.

[0036] Embodiment 2

[0037] S1, adding 20 parts of o-cresol type novolac epoxy resin to 47.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, recorded as the first mixed system;

[0038] S2, add 1-aminoethyl-3-methylimidazolium cation to water, add hexafluorophosphate anion in batches under stirring, adjust the pH to 6-7 by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add 7.5 parts of the prepared ion gel and 7.5 parts of 5% sodium silicate gel to the first mixed system obtained in step S1, stir and dissolve, and record as the second mixed system;

[0039] S3, adding beeswax to a diluent, heating to melt, dropping 2M sodium carbonate solution, adjusting the pH to 7-8, and cooling to obtain modified beeswax; adding 1.75 parts of modified beeswax and 2.75 parts of glass fiber to the second mixed system obtained in step S2, stirring to dissolve, and recording as the third mixed system;

[0040] S4, adding 7 parts of organosilicon-modified polyacrylic acid resin to 12.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, and recording as the fourth mixing system;

[0041] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0042] S6, suspend 0.75 parts of potassium carbonate powder in catechol, add oxalic acid to adjust pH≈1 under stirring, stir at room temperature for 4 hours, filter, add the filtrate to the fifth mixed system obtained in step S5, stir and mix, and record it as the sixth mixed system

[0043] S7. The sixth mixed system is coated on the surface of the PET base film by atomizing spraying, and then aged under ultraviolet light to obtain an anti-warping core layer with a thickness of 180 μm.

[0044] Embodiment 3

[0045] S1, adding 25 parts of o-cresol type novolac epoxy resin to 50 parts of resorcinol bisglycidyl ether, stirring to dissolve, recorded as the first mixed system;

[0046] S2, add 1-aminoethyl-3-methylimidazolium cation to water, add hexafluorophosphate anion in batches under stirring, adjust the pH to 6-7 by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add 10 parts of the prepared ion gel and 10 parts of 5% sodium silicate gel to the first mixed system obtained in step S1, stir and dissolve, and record as the second mixed system;

[0047] S3, adding beeswax to a diluent, heating to melt, dropping 2M sodium carbonate solution, adjusting the pH to 7-8, and cooling to obtain modified beeswax; adding 3 parts of modified beeswax and 5 parts of glass fiber to the second mixed system obtained in step S2, stirring to dissolve, and recording as the third mixed system;

[0048] S4, adding 10 parts of organosilicon-modified polyacrylic acid resin to 15 parts of resorcinol bisglycidyl ether, stirring to dissolve, and recording as the fourth mixing system;

[0049] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0050] S6. Suspend 1 portion of potassium carbonate powder in catechol, add oxalic acid to adjust pH≈1 under stirring, stir at room temperature for 4 hours, filter, add the filtrate to the fifth mixed system obtained in step S5, stir and mix, and record it as the sixth mixed system

[0051] S7. The sixth mixed system is coated on the surface of the PET base film by atomizing spraying, and then aged under ultraviolet light to obtain an anti-warping core layer with a thickness of 210 μm.

[0052] Comparative Example 1

[0053] S1, adding 20 parts of o-cresol type novolac epoxy resin to 47.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, recorded as the first mixed system;

[0054] S2, add 1-aminoethyl-3-methylimidazolium cation to water, add hexafluorophosphate anion in batches under stirring, adjust the pH to 6-7 by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add 7.5 parts of the prepared ion gel and 7.5 parts of 5% sodium silicate gel to the first mixed system obtained in step S1, stir and dissolve, and record as the second mixed system;

[0055] S3, adding beeswax to a diluent, heating to melt, dropping 2M sodium carbonate solution, adjusting the pH to 7-8, and cooling to obtain modified beeswax; adding 1.75 parts of modified beeswax and 2.75 parts of glass fiber to the second mixed system obtained in step S2, stirring to dissolve, and recording as the third mixed system;

[0056] S4, adding 7 parts of organosilicon-modified polyacrylic acid resin to 12.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, and recording as the fourth mixing system;

[0057] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0058] S6, suspend 0.75 parts of potassium carbonate powder in catechol, add oxalic acid to adjust pH≈1 under stirring, stir at room temperature for 4 hours, filter, add the filtrate to the fifth mixed system obtained in step S5, stir and mix, and record it as the sixth mixed system

[0059] S7. The sixth mixed system is coated on the surface of the PET base film by atomizing spraying, and then aged under ultraviolet light to obtain an anti-warping core layer with a thickness of 180 μm.

[0060] Comparative Example 2

[0061] S1, adding 20 parts of o-cresol type novolac epoxy resin to 47.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, recorded as the first mixed system;

[0062] S2, add 1-aminoethyl-3-methylimidazolium cation to water, add hexafluorophosphate anion in batches under stirring, adjust the pH to 6-7 by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add 7.5 parts of the prepared ion gel and 7.5 parts of 5% sodium silicate gel to the first mixed system obtained in step S1, stir and dissolve, and record as the second mixed system;

[0063] S3, adding 2.75 parts of glass fiber to the second mixed system obtained in step S2, stirring and dissolving, and recording as the third mixed system;

[0064] S4, adding 7 parts of organosilicon-modified polyacrylic acid resin to 12.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, and recording as the fourth mixing system;

[0065] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0066] S6, suspend 0.75 parts of potassium carbonate powder in catechol, add oxalic acid to adjust pH≈1 under stirring, stir at room temperature for 4 hours, filter, add the filtrate to the fifth mixed system obtained in step S5, stir and mix, and record it as the sixth mixed system

[0067] S7. The sixth mixed system is coated on the surface of the PET base film by atomizing spraying, and then aged under ultraviolet light to obtain an anti-warping core layer with a thickness of 180 μm.

[0068] Comparative Example 3

[0069] S1, adding 20 parts of o-cresol type novolac epoxy resin to 47.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, recorded as the first mixed system;

[0070] S2, add 1-aminoethyl-3-methylimidazolium cation to water, add hexafluorophosphate anion in batches under stirring, adjust the pH to 6-7 by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add 7.5 parts of the prepared ion gel to the first mixed system obtained in step S1, stir and dissolve, and record it as the second mixed system;

[0071] S3, adding beeswax to a diluent, heating to melt, dropping 2M sodium carbonate solution, adjusting the pH to 7-8, and cooling to obtain modified beeswax; adding 1.75 parts of modified beeswax and 2.75 parts of glass fiber to the second mixed system obtained in step S2, stirring to dissolve, and recording as the third mixed system;

[0072] S4, adding 7 parts of organosilicon-modified polyacrylic acid resin to 12.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, and recording as the fourth mixing system;

[0073] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0074] S6. The fifth mixed system is coated on the surface of the PET base film by atomizing spraying, and then aged under ultraviolet light to obtain an anti-warping core layer with a thickness of 180 μm.

[0075] Comparative Example 4

[0076] S1, adding 20 parts of o-cresol type novolac epoxy resin to 47.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, recorded as the first mixed system;

[0077] S2, add 1-aminoethyl-3-methylimidazolium cation to water, add hexafluorophosphate anion in batches under stirring, adjust the pH to 6-7 by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add 7.5 parts of the prepared ion gel and 7.5 parts of 5% sodium silicate gel to the first mixed system obtained in step S1, stir and dissolve, and record as the second mixed system;

[0078] S3, adding 2.75 parts of glass fiber to the second mixed system obtained in step S2, stirring and dissolving, and recording as the third mixed system;

[0079] S4, adding 7 parts of organosilicon-modified polyacrylic acid resin to 12.5 parts of resorcinol bisglycidyl ether, stirring to dissolve, and recording as the fourth mixing system;

[0080] S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system;

[0081] S6. The fifth mixed system is coated on the surface of the PET base film by atomizing spraying, and then aged under ultraviolet light to obtain an anti-warping core layer with a thickness of 180 μm.

[0082] Test method:

[0083] 1. Heat shrinkage rate: Cut the sample to be tested into 20cm×20cm pieces, use an image measuring instrument to measure the size S1 of the sample before heat treatment, place the sample in an oven, set the temperature to 85℃, start timing when the temperature reaches 85℃, take out the sample after 30 minutes, cool it to room temperature, and use an image measuring instrument to measure the size S2 of the sample after heat treatment. The calculation formula is: (S1-S2) / S1×100%.

[0084] 2. Thermal expansion coefficient: Cut the sample to be tested into 20mm×5mm samples, use thermal expansion coefficient tester (TMA7300 thermomechanical analyzer), load 22.05mN, test range 20-85℃ (ΔT=65℃), heating rate 10℃ / min, the dimensional change in this temperature range is ΔL, and the calculation formula is α=ΔL / (L×ΔT).

[0085] 3. Stiffness test: refer to GB / T 23144-2008 "General Principles for Determination of Static Bending Stiffness of Paper and Paperboard". During the test, fix one end of the sample on the rotating head, and hold the other end of the film with the stringer. Then, when the rotating head rotates 15°, keep it for 5s, and the torque value obtained by the sensor, the unit of the torque value is mN·m, which is the measured value of the stiffness. The larger the torque value, the better the stiffness of the brightening film.

[0086] 4. Warpage test: Cut the sample to be tested into 100mm×100mm pieces, and then place them in an environment of 65℃ and 95%RH for 240h. Then naturally cool them to room temperature. Take out the pieces and place them on a horizontal platform to measure the warpage height.

[0087]

[0088] By comparing the experimental data, it can be seen that the thermal shrinkage rate, thermal expansion coefficient, and warpage value of the embodiments all show good performance. The warpage values ​​of the embodiments are all less than 1 mm and below 0.7 mm, and the anti-warpage performance is significantly improved.

[0089] Of course, the above description is not a limitation of the present invention. The above description is only a preferred example of the invention. Any changes, modifications, additions or substitutions made according to the content of the present invention are covered by the patent scope of the present invention.

Claims

1. A warping-resistant core layer, characterized in that: The base film is coated with a prepared anti-warping solution, which includes the following components: epoxy resin, curing agent, ion gel, silica gel, modified beeswax, anti-compression hardener, filler, and diluent.

2. The anti-warping core layer according to claim 1, characterized in that: The substrate layer is a PET base film.

3. The anti-warping core layer according to claim 1, characterized in that: The thickness of the anti-warping core layer is 150-210 μm.

4. The anti-warping core layer according to claim 1, characterized in that: The anti-warping solution comprises the following components by weight: 15 to 25 parts of epoxy resin, 4 to 10 parts of curing agent, 5 to 10 parts of ion gel, 5 to 10 parts of silica gel, 0.5 to 3 parts of modified beeswax, 0.5 to 5 parts of filler, 0.5 to 1 part of anti-compression hardener, and 55 to 65 parts of diluent.

5. The anti-warping core layer according to claim 1, characterized in that: The epoxy resin includes at least one of hydrogenated bisphenol A diglycidyl ether, phenol-type novolac epoxy resin, and o-cresol-type novolac epoxy resin; The curing agent includes at least one of polyvinyl ester resin, polyacrylic acid resin, and organosilicon-modified polyacrylic acid resin; The ion gel is obtained by polymerizing an imidazole cationic liquid monomer and an acid radical or imide anionic liquid monomer, wherein the imidazole cationic liquid monomer is at least one of 1-aminopropyl-3-methylimidazolium cation, 1-aminoethyl-3-methylimidazolium cation, 1-vinyl-3-methylimidazolium cation, and 1-decyl-3-methylimidazolium cation; and the acid radical or imide anionic liquid monomer is at least one of tetrafluoroborate anion, hexafluorophosphate anion, and bistrifluoromethanesulfonyl imide anion. The silicic acid gel includes at least one of 3% sodium silicate gel, 5% sodium silicate gel, and 7% sodium silicate; The modified beeswax includes at least one of modified Chinese beeswax and modified Western beeswax; The filler includes any one of white carbon black, glass fiber, and precipitated barium sulfate; The compressive hardener is a potassium tantalate ternary complex, which is prepared by suspending potassium carbonate powder in catechol, adding oxalic acid to adjust the pH to 1 under stirring, and stirring at room temperature for 4 hours; The diluent includes any one of resorcinol diglycidyl ether, β-hydroxyethyl methacrylate, 1,6-hexanediol diacrylate, and polypropylene glycol diglycidyl ether.

6. A method for preparing an anti-warping core layer according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, adding the formulated amount of epoxy resin into the diluent, stirring to dissolve, and recording as the first mixed system; S2, add cations to water, add anions in batches under stirring, adjust pH by ultrasonic heating, filter, slurry with ethanol, filter and dry to obtain ion gel. Add the formulated amount of ion gel and silica gel to the first mixed system obtained in step S1, stir and dissolve, and record it as the second mixed system; S3, adding beeswax to a diluent, heating to melt, dropping a sodium carbonate solution, adjusting the pH, and cooling to obtain modified beeswax; Adding the modified beeswax and filler in the formula amount to the second mixed system obtained in step S2, stirring and dissolving, and recording as the third mixed system; S4, adding the formulated amount of curing agent to the diluent, stirring and dissolving, and recording as the fourth mixing system; S5, slowly adding the fourth mixed system to the third mixed system obtained in step S4, stirring and mixing, which is recorded as the fifth mixed system; S6, suspending potassium carbonate powder in catechol, adding oxalic acid to adjust pH≈1 under stirring, stirring at room temperature for 4 hours, filtering, and adding the filtrate to the fifth mixed system obtained in step S5, stirring and mixing, and recording as the sixth mixed system S7. Prepare a base film, apply the sixth mixed system on the upper surface of the substrate layer by atomizing spraying, ultrasonic spraying, or anilox roller coating, and then age it under ultraviolet light to obtain an anti-warping core layer with a thickness of 150 to 210 μm.