Modified isotatic polypropylene as well as preparation method and application thereof
By using polyetherester thermoplastic polyester elastomer modified polypropylene in 3D printing materials, the problems of high warpage and poor dimensional stability of polypropylene products are solved, and low shrinkage warpage and high impact resistance are achieved, satisfying the industry Application accuracy and strength requirements.
Patent Information
- Application Number
- CN202411155722.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
Polypropylene products in existing 3D printing materials have problems such as excessive warping and poor dimensional stability, which is difficult to meet the requirements of precision and strength in industrial applications.
Modified by polyether ester thermoplastic polyester elastomer (TPEE) and polypropylene, and modified isotropic polypropylene is prepared by melt blending and extrusion, improving the spatial arrangement compactness and adhesion of the material, reducing shrinkage warping and Improve impact resistance.
It significantly improves the dimensional stability and warping resistance of the product, meets the requirements of product accuracy and strength in industrial applications, and solves the problems of high warping and poor dimensional stability.
Smart Images

Figure BDA0005009646380000011 
Figure BDA0005009646380000031 
Figure BDA0005009646380000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of 3D printing materials, and specifically relates to a modified isotactic polypropylene and a preparation method and application thereof. Background Art
[0002] 3D printing generally uses a computer to control a 3D printer, stacking the printing materials in the 3D printer layer by layer to turn the blueprint into a three-dimensional object. The most common method of 3D printing is fused deposition modeling, but the printing materials that can be used are relatively small, so the printing materials have become the main factor restricting the fused deposition modeling process and the performance of the finished product.
[0003] At present, common printing materials include polylactic acid and acrylonitrile-butadiene-styrene copolymer, but their mechanical properties are poor. In addition, polypropylene is also a commonly used printing material, which solves the problem of poor mechanical properties of printing materials such as polylactic acid. However, when it is used as a printing material, there are problems such as severe warping and deformation of molded products and poor dimensional stability, which cannot meet the requirements of industrial applications for the precision of polypropylene printed products.
[0004] Chinese patent CN108641197A discloses a polypropylene wire for 3D printing and a preparation method thereof. The composite material includes copolymer polypropylene, low melting point homopolymer polypropylene, inorganic filler, thermoplastic elastomer, plasticizer and stabilizer. The composite material can be used for 3D printing, but there are still problems of excessive warpage and poor dimensional stability of the product. Summary of the invention
[0005] The purpose of the present invention is to provide a modified isotactic polypropylene and a preparation method and application thereof. The modified isotactic polypropylene provided by the present invention has low shrinkage warpage, high impact resistance and good dimensional stability.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a modified isotactic polypropylene, which is prepared from raw materials including the following components in parts by mass:
[0008] 30-60 parts of polypropylene, 40-70 parts of polyether ester thermoplastic polyester elastomer, 10-30 parts of compatibilizer and 1-10 parts of antioxidant.
[0009] Preferably, the polypropylene is polypropylene 1102K.
[0010] Preferably, the polyetherester thermoplastic polyester elastomer is a compound represented by Formula I:
[0011]
[0012] In formula I, m:n=6:4;
[0013] The weight average molecular weight of the polyether ester thermoplastic polyester elastomer is 1000-6000.
[0014] Preferably, the compatibilizer is glycidyl methacrylate grafted polypropylene.
[0015] Preferably, the antioxidant is antioxidant 1010.
[0016] The present invention also provides a method for preparing the modified isotactic polypropylene described in the above scheme, comprising the following steps:
[0017] Polypropylene, polyether ester thermoplastic polyester elastomer, compatibilizer and antioxidant are mixed and then melt-blended and extruded. The melt-blending and extrusion are performed for more than 2 times to obtain modified isotactic polypropylene.
[0018] Preferably, the melt blending and extrusion is performed 2 to 4 times.
[0019] Preferably, the temperature of the melt blending extrusion is 210-220°C, the screw speed is 30-50 rpm, and the holding time is 10-15 s. 。
[0020] Preferably, the equipment for melt blending extrusion is a twin-screw extruder; the twin-screw extruder is divided into one to three zones; the temperature of the one zone is 120-130°C, and the insulation time is 0-5s and is not 0; the temperature of the two zones is 170-180°C, and the insulation time is 0-5s and is not 0; the temperature of the three zones is 190-200°C, and the insulation time is 0-5s and is not 0.
[0021] The present invention also provides the use of the modified isotactic polypropylene described in the above scheme or the modified isotactic polypropylene obtained by the preparation method described in the above scheme in 3D printing.
[0022] The present invention provides a modified isotactic polypropylene. The present invention uses polyether ester thermoplastic polyester elastomer (TPEE) to modify polypropylene (PP): on the one hand, the soft segment of TPEE has a spatial coordination effect, making the spatial arrangement of PP molecular chains more compact, thereby reducing the crystallinity, and thus significantly improving the dimensional stability and warpage resistance of the product, thereby meeting the requirements of industrial applications for product precision and strength; on the other hand, TPEE has a certain polarity, which can improve the adhesion between the material and the printing platform. The modified isotactic polypropylene provided by the present invention has low shrinkage warpage and high impact resistance, good dimensional stability, and solves the problems of excessive warpage and poor dimensional stability of existing 3D printed products made of polypropylene materials.
[0023] The present invention also provides a method for preparing the modified isotactic polypropylene described in the above scheme. The present invention prepares the modified isotactic polypropylene by melt blending and extrusion, which has low shrinkage warpage and high impact resistance, greatly improves comprehensive performance, and can be used for 3D printing.
[0024] The present invention also provides the use of the modified isotactic polypropylene described in the above scheme or the modified isotactic polypropylene obtained by the preparation method described in the above scheme in 3D printing. The modified isotactic polypropylene provided by the present invention can be used for 3D printing to obtain 3D products with low shrinkage warpage and good dimensional stability. DETAILED DESCRIPTION
[0025] The present invention provides a modified isotactic polypropylene, which is prepared from raw materials including the following components in parts by mass:
[0026] 30-60 parts of polypropylene, 40-70 parts of polyether ester thermoplastic polyester elastomer, 10-30 parts of compatibilizer and 1-10 parts of antioxidant.
[0027] The raw material of the modified isotactic polypropylene provided by the present invention comprises 30 to 60 parts of polypropylene, preferably 35 to 60 parts, more preferably 45 to 55 parts, and further preferably 50 parts.
[0028] In the present invention, the polypropylene is preferably polypropylene 1102K.
[0029] The raw material of the modified isotactic polypropylene provided by the present invention comprises 40 to 70 parts of polyether ester thermoplastic polyester elastomer, preferably 40 to 65 parts, more preferably 40 to 60 parts, and further preferably 45 to 55 parts.
[0030] In the present invention, the polyether ester thermoplastic polyester elastomer is preferably a compound represented by formula I:
[0031]
[0032] In formula I, m:n=6:4;
[0033] The weight average molecular weight of the polyetherester thermoplastic polyester elastomer is preferably 1000-6000, more preferably 2000-4000.
[0034] In a specific embodiment of the present invention, the polyether ester thermoplastic polyester elastomer is preferably H2040 polyether ester thermoplastic polyester elastomer.
[0035] The raw material of the modified isotactic polypropylene provided by the present invention comprises 10 to 30 parts of a compatibilizer, preferably 15 to 25 parts, more preferably 17 to 23 parts, and further preferably 20 parts.
[0036] In the present invention, the compatibilizer is preferably glycidyl methacrylate grafted polypropylene (PP-g-GMA).
[0037] The raw material of the modified isotactic polypropylene provided by the present invention comprises 1 to 10 parts of antioxidant, preferably 3 to 7 parts, more preferably 4 to 6 parts, and further preferably 5 parts.
[0038] In the present invention, the antioxidant is preferably antioxidant 1010.
[0039] The present invention also provides a method for preparing the modified isotactic polypropylene described in the above scheme, comprising the following steps:
[0040] Polypropylene, polyether ester thermoplastic polyester elastomer, compatibilizer and antioxidant are mixed and then melt-blended and extruded. The melt-blending and extrusion are performed for more than 2 times to obtain modified isotactic polypropylene.
[0041] The present invention mixes polypropylene, polyether ester thermoplastic polyester elastomer, a compatibilizer and an antioxidant (referred to as the first mixing). In the present invention, the first mixing is preferably stirring mixing; the rotation speed of the stirring mixing is preferably 50 to 90 rpm, more preferably 60 to 80 rpm, and further preferably 70 rpm; the stirring time is preferably 6 to 10 min, more preferably 7 to 9 min, and further preferably 8 min; the stirring mixing device is preferably a high-speed stirrer.
[0042] After mixing, a mixed material is obtained, and the mixed material is melt-blended and extruded in the present invention, and the melt-blending and extrusion are performed for more than 2 times to obtain modified isotactic polypropylene. In the present invention, the melt-blending and extrusion are performed for preferably 2 to 4 times, and more preferably 3 times.
[0043] In the present invention, the equipment for melt blending and extrusion is preferably a twin-screw extruder; the temperature of the melt blending and extrusion is preferably 210-220°C, more preferably 213-217°C, and further preferably 215°C; the screw speed is preferably 30-50rpm, more preferably 35-45rpm, and further preferably 40rpm; the holding time is preferably 10-15s, more preferably 11-14s, and further preferably 13s.
[0044] In the present invention, the twin-screw extruder is preferably divided into one to three zones; the temperature of the one zone is preferably 120-130°C, more preferably 125°C, and the insulation time is preferably 0-5s and not 0, more preferably 3s; the temperature of the second zone is preferably 170-180°C, more preferably 175°C, and the insulation time is preferably 0-5s and not 0, more preferably 3s; the temperature of the third zone is preferably 190-200°C, more preferably 195°C, and the insulation time is preferably 0-5s and not 0, more preferably 3s.
[0045] In the present invention, after the melt blending extrusion, it is preferred that the obtained products are collected into filaments and granulated in sequence; the granulation is preferably cut into granules; the particle size of the granules is preferably 1 to 3 mm, more preferably 1.5 to 2.5 mm, and further preferably 1.5 to 2 mm; the equipment for cutting into granules is preferably a pelletizer.
[0046] The present invention also provides the use of the modified isotactic polypropylene described in the above scheme or the modified isotactic polypropylene obtained by the preparation method described in the above scheme in 3D printing.
[0047] The modified isotactic polypropylene provided by the present invention can be used for 3D printing to obtain 3D products with low shrinkage, warping and good dimensional stability.
[0048] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0049] Example 1
[0050] The method for preparing modified isotactic polypropylene in this embodiment comprises the following steps:
[0051] Weigh the raw materials according to the following mass parts: 30 parts of 1102K polypropylene, 70 parts of H2040 polyether ester thermoplastic polyester elastomer, 10 parts of PP-g-GMA compatibilizer, and 1 part of 1010 antioxidant;
[0052] The weighed raw materials are sequentially added into a high-speed mixer, stirred at a high speed for 8 minutes, and mixed evenly; the mixed raw materials are melt-blended and extruded using a twin-screw extruder (the twin-screw extruder is divided into one to three zones, the temperature of the first zone is 125° C., the insulation time is 3 seconds, the temperature of the second zone is 175° C., the insulation time is 3 seconds, and the temperature of the third zone is 195° C., the insulation time is 3 seconds), and the raw materials are passed through the outlet die of the extruder, collected into filaments, and then cut by a pelletizer, and the formed particles are collected to obtain particles of modified isotactic polypropylene; and the particles of the isotactic polypropylene are secondary blended, collected into filaments, and pelletized to obtain modified isotactic polypropylene.
[0053] Example 2
[0054] The method for preparing modified isotactic polypropylene in this embodiment comprises the following steps:
[0055] The raw materials were weighed according to the following mass proportions: 50 parts of 1102K polypropylene, 50 parts of H2040 polyether ester thermoplastic polyester elastomer, 10 parts of PP-g-GMA compatibilizer, and 1 part of 1010 antioxidant.
[0056] The weighed raw materials are sequentially added into a high-speed mixer, stirred at a high speed for 8 minutes, and mixed evenly; the mixed raw materials are melt-blended and extruded using a twin-screw extruder (the twin-screw extruder is divided into one to three zones, the temperature of the first zone is 125° C., the insulation time is 3 seconds, the temperature of the second zone is 175° C., the insulation time is 3 seconds, and the temperature of the third zone is 195° C., the insulation time is 3 seconds), and the raw materials are passed through the outlet die of the extruder, collected into filaments, and then cut by a pelletizer, and the formed particles are collected to obtain particles of modified isotactic polypropylene; and the particles of the isotactic polypropylene are secondary blended, collected into filaments, and pelletized to obtain modified isotactic polypropylene.
[0057] Example 3
[0058] The method for preparing modified isotactic polypropylene in this embodiment comprises the following steps:
[0059] The raw materials were weighed according to the following mass proportions: 60 parts of 1102K polypropylene, 40 parts of H2040 polyether ester thermoplastic polyester elastomer, 10 parts of PP-g-GMA compatibilizer, and 1 part of 1010 antioxidant.
[0060] The weighed raw materials are sequentially added into a high-speed mixer, stirred at a high speed for 8 minutes, and mixed evenly; the mixed raw materials are melt-blended and extruded using a twin-screw extruder (the twin-screw extruder is divided into one to three zones, the temperature of the first zone is 125° C., the insulation time is 3 seconds, the temperature of the second zone is 175° C., the insulation time is 3 seconds, and the temperature of the third zone is 195° C., the insulation time is 3 seconds), and the raw materials are passed through the outlet die of the extruder, collected into filaments, and then cut by a pelletizer, and the formed particles are collected to obtain particles of modified isotactic polypropylene; and the particles of the isotactic polypropylene are secondary blended, collected into filaments, and pelletized to obtain modified isotactic polypropylene.
[0061] Comparative Example 1
[0062] The method for preparing modified isotactic polypropylene in this embodiment comprises the following steps:
[0063] The raw materials were weighed according to the following mass proportions: 70 parts of 1102K polypropylene, 30 parts of H2040 polyether ester thermoplastic polyester elastomer, 10 parts of PP-g-GMA compatibilizer, and 1 part of 1010 antioxidant.
[0064] The weighed raw materials are sequentially added into a high-speed mixer, stirred at a high speed for 8 minutes, and mixed evenly; the mixed raw materials are melt-blended and extruded using a twin-screw extruder (the twin-screw extruder is divided into one to three zones, the temperature of the first zone is 125° C., the insulation time is 3 seconds, the temperature of the second zone is 175° C., the insulation time is 3 seconds, and the temperature of the third zone is 195° C., the insulation time is 3 seconds), and the raw materials are passed through the outlet die of the extruder, collected into filaments, and then cut by a pelletizer, and the formed particles are collected to obtain particles of modified isotactic polypropylene; and the particles of the isotactic polypropylene are secondary blended, collected into filaments, and pelletized to obtain modified isotactic polypropylene.
[0065] Comparative Example 2
[0066] The method for preparing modified isotactic polypropylene in this embodiment comprises the following steps:
[0067] The raw materials were weighed according to the following mass proportions: 50 parts of 1102K polypropylene, 50 parts of H3030 thermoplastic polyester elastomer, 10 parts of PP-g-GMA compatibilizer, and 1 part of 1010 antioxidant.
[0068] The polyether ester thermoplastic polyester elastomer is a compound shown in Formula II:
[0069]
[0070] In formula II, m:n=7:3.
[0071] The weighed raw materials are sequentially added into a high-speed mixer, stirred at a high speed for 8 minutes, and mixed evenly; the mixed raw materials are melt-blended and extruded using a twin-screw extruder (the twin-screw extruder is divided into one to three zones, the temperature of the first zone is 125° C., the insulation time is 3 seconds, the temperature of the second zone is 175° C., the insulation time is 3 seconds, and the temperature of the third zone is 195° C., the insulation time is 3 seconds), and the raw materials are passed through the outlet die of the extruder, collected into filaments, and then cut by a pelletizer, and the formed particles are collected to obtain particles of modified isotactic polypropylene; and the particles of the isotactic polypropylene are secondary blended, collected into filaments, and pelletized to obtain modified isotactic polypropylene.
[0072] Comparative Example 3
[0073] The method for preparing modified isotactic polypropylene in this embodiment comprises the following steps:
[0074] The raw materials were weighed according to the following mass proportions: 50 parts of 1102K polypropylene, 50 parts of H7560 thermoplastic polyester elastomer, 10 parts of PP-g-GMA compatibilizer, and 1 part of 1010 antioxidant.
[0075] The polyether ester thermoplastic polyester elastomer is a compound represented by formula III:
[0076]
[0077] In formula III, m:n=11:9.
[0078] The weighed raw materials are sequentially added into a high-speed mixer, stirred at a high speed for 8 minutes, and mixed evenly; the mixed raw materials are melt-blended and extruded using a twin-screw extruder (the twin-screw extruder is divided into one to three zones, the temperature of the first zone is 125° C., the insulation time is 3 seconds, the temperature of the second zone is 175° C., the insulation time is 3 seconds, and the temperature of the third zone is 195° C., the insulation time is 3 seconds), and the raw materials are passed through the outlet die of the extruder, collected into filaments, and then cut by a pelletizer, and the formed particles are collected to obtain particles of modified isotactic polypropylene; and the particles of the isotactic polypropylene are secondary blended, collected into filaments, and pelletized to obtain modified isotactic polypropylene.
[0079] Comparative Example 4
[0080] The method for preparing modified isotactic polypropylene in this embodiment comprises the following steps:
[0081] The raw materials were weighed according to the following mass proportions: 50 parts of 1102K polypropylene, 50 parts of H5550 thermoplastic polyester elastomer, 10 parts of PP-g-GMA compatibilizer, and 1 part of 1010 antioxidant.
[0082] The polyether ester thermoplastic polyester elastomer is a compound represented by formula IV:
[0083]
[0084] In formula IV, m:n=5:5.
[0085] The weighed raw materials are sequentially added into a high-speed mixer, stirred at a high speed for 8 minutes, and mixed evenly; the mixed raw materials are melt-blended and extruded using a twin-screw extruder (the twin-screw extruder is divided into one to three zones, the temperature of the first zone is 125° C., the insulation time is 3 seconds, the temperature of the second zone is 175° C., the insulation time is 3 seconds, and the temperature of the third zone is 195° C., the insulation time is 3 seconds), and the raw materials are passed through the outlet die of the extruder, collected into filaments, and then cut by a pelletizer, and the formed particles are collected to obtain particles of modified isotactic polypropylene; and the particles of the isotactic polypropylene are secondary blended, collected into filaments, and pelletized to obtain modified isotactic polypropylene.
[0086] Test Case
[0087] The modified isotactic polypropylene prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was subjected to performance tests, wherein the impact strength was tested using the GB / T1843-1996 test standard.
[0088] The modified isotactic polypropylene prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4 was used as a 3D printing material, and a fused deposition modeling (FGF) process was adopted to print the modified isotactic polypropylene particles into performance test samples through a 3D printing device; wherein the printing conditions of the fused deposition modeling were: a layer thickness of 0.4 mm, a nozzle temperature of 260° C., and a hot stage temperature of 75° C.
[0089] Table 1 Performance test results of Examples 1 to 3 and Comparative Examples 1 to 4
[0090]
[0091]
[0092] It can be seen from Table 1 that the modified isotactic polypropylene provided by the present invention has a low warpage, which can be as low as 2.9%, and has good impact strength and guaranteed mechanical properties.
[0093] It can be seen from the above embodiments that the performance of the modified isotactic polypropylene provided by the present invention is greatly improved, and the warpage can well solve the problem of serious warping and deformation of polypropylene material products, and meet the requirements of industrial applications for product precision and strength.
[0094] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A modified isotactic polypropylene, characterized in that: According to the mass fraction, it is prepared from the raw materials including the following components: 30-60 parts of polypropylene, 40-70 parts of polyether ester thermoplastic polyester elastomer, 10-30 parts of compatibilizer and 1-10 parts of antioxidant.
2. The modified isotactic polypropylene according to claim 1, characterized in that: The polypropylene is polypropylene 1102K.
3. The modified isotactic polypropylene according to claim 1 or 2, characterized in that: The polyether ester thermoplastic polyester elastomer is a compound shown in Formula I: In formula I, m:n=6:4; The weight average molecular weight of the polyether ester thermoplastic polyester elastomer is 1000-6000.
4. The modified isotactic polypropylene according to claim 1, characterized in that: The compatibilizer is glycidyl methacrylate grafted polypropylene.
5. The modified isotactic polypropylene according to claim 1 or 4, characterized in that: The antioxidant is antioxidant 1010.
6. The method for preparing modified isotactic polypropylene according to any one of claims 1 to 5, characterized in that: The following steps are involved: Polypropylene, polyether ester thermoplastic polyester elastomer, compatibilizer and antioxidant are mixed and then melt-blended and extruded. The melt-blending and extrusion are performed for more than 2 times to obtain modified isotactic polypropylene.
7. The preparation method according to claim 6, characterized in that: The melt blending and extrusion is performed 2 to 4 times.
8. The preparation method according to claim 6 or 7, characterized in that: The temperature of the melt blending extrusion is 210-220° C., the screw speed is 30-50 rpm, and the heat preservation time is 10-15 s.
9. The preparation method according to claim 6, characterized in that: The equipment for melt blending extrusion is a twin-screw extruder; the twin-screw extruder is divided into one to three zones; the temperature of the one zone is 120-130°C, the insulation time is 0-5s and is not 0; the temperature of the two zones is 170-180°C, the insulation time is 0-5s and is not 0; the temperature of the three zones is 190-200°C, the insulation time is 0-5s and is not 0.
10. Use of the modified isotactic polypropylene according to any one of claims 1 to 5 or the modified isotactic polypropylene obtained by the preparation method according to any one of claims 6 to 9 in 3D printing.