Longitudinal and transverse wood fiber balance artificial board and production process thereof

Through the production process of vertical and horizontal vertical wood fiber balanced artificial boards, the interwoven fiber network is formed by using rotary cutting and lamination processes, and combined with modified lignin adhesive, the problems of easy deformation and warping of traditional wood balanced boards are solved, achieving higher mechanical properties and structural stability.

CN118952399AActive Publication Date: 2024-11-15JIANGSU QINGYUN WOOD IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411256453.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

Traditional wooden balance boards are prone to deformation and warping, limiting the application range of the board.

Method used

The production process of vertical and horizontal vertical wood fiber balanced artificial boards is adopted, and an interwoven wood fiber network is formed through rotary cutting and lamination processes, and a modified lignin adhesive is used to improve the mechanical properties and waterproofness of the board.

Benefits of technology

It significantly improves the mechanical strength and structural stability of the board, improves stiffness and warping resistance, while maintaining excellent bonding and waterproofness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a longitudinal and transverse wood fiber balance artificial board and a production process thereof, and belongs to the technical field of solid wood composite boards. According to the artificial board, logs are subjected to rotary cutting to obtain slices with oriented wood fibers, the slices are longitudinally laminated and glued to form square stocks with good machinability, the slices are longitudinally flaked and rotationally laminated, so that the wood fibers are crisscrossed, an interlaced wood fiber network is formed in space, stress is uniformly dispersed when the wood fibers are subjected to external force, and the wood fibers are uniformly dispersed; the plate has higher mechanical strength and structural stability, and the rigidity and warping resistance of the plate are remarkably improved in a test; the slices are bonded through a lignin adhesive, the lignin adhesive takes a traditional PMDI prepolymer as a gluing matrix, and independently researched and developed modified lignin is introduced to improve the water resistance of an adhesive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid wood composite panels, and in particular relates to a vertical and horizontal wood fiber balanced artificial board and a production process thereof. Background Art

[0002] Traditional wooden balance boards are made of solid wood, which has low wood utilization and high prices. With the advancement of science and technology and the innovation of technology, multi-layer artificial boards are often used as substitutes in existing technologies, which not only reduce costs but also allow for diversified designs according to needs. Artificial boards are highly favored due to their unique advantages. However, multi-layer artificial boards are prone to deformation and warping, which seriously limits the application of boards. Summary of the invention

[0003] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a vertical and horizontal wood fiber balanced artificial board and a production process thereof.

[0004] The purpose of the present invention can be achieved by the following technical solutions:

[0005] A production process of a vertical and horizontal wood fiber balanced artificial board, comprising the following steps:

[0006] Step S1: the log is peeled and the slices are dried, and then lignin adhesive is applied in sequence, the slices are longitudinally stacked and pressurized to obtain square materials;

[0007] Step S2: Plane the square material longitudinally to form green sheets, rotate adjacent green sheets longitudinally, and then sequentially coat the green sheets with lignin adhesive, transversely stack and press-cure to obtain vertical and horizontal wood fiber balanced artificial boards.

[0008] Preferably, the longitudinal rotation angle is 90°. In this state, the wood fibers of the blank are easy to form a uniform vertical structure in the longitudinal and transverse directions, which is beneficial to improving the stability of the mechanical properties of the board.

[0009] The lignin adhesive comprises, by weight: 100 parts of PMDI prepolymer, 18-26 parts of modified lignin, 5-8 parts of metal oxide filler, 0.4-0.5 parts of leveling agent and 10-15 parts of diluent.

[0010] Preferably, the -NCO content of the PMDI prepolymer is 30-35%, and the adhesive formulated in this state has good coatability and curing activity.

[0011] Preferably, the metal oxide filler is one or more of zinc oxide, titanium oxide and aluminum oxide, which can be chelated and strengthened with the modified lignin and have good antibacterial and anti-mildew effects.

[0012] The modified lignin is prepared by the following method:

[0013] Step A1: ultrasonically disperse lignin, tetrafluorobutanediol and anhydrous dioxane, introduce dry nitrogen for protection, heat to 85-95°C, stir at 90-120 rpm, intermittently add methylvinyldichlorosilane to react for 5-7 hours, and remove dioxane by rotary evaporation after the reaction to obtain fluorosilicified lignin;

[0014] Furthermore, the dosage ratio of lignin, tetrafluorobutanediol, methylvinyldichlorosilane and anhydrous dioxane is 50g:15-20mmol:30-40mmol:80-100mL, and the highly active methylvinyldichlorosilane reacts with the hydroxyl groups on the lignin molecules and tetrafluorobutanediol to introduce fluorine-silicon structures and unsaturated double bonds into the lignin molecules.

[0015] Step A2: Premix fluorosilicified lignin, benzoin dimethyl ether and dimethylacetamide by ultrasonication, pass nitrogen protection, add mercaptoethanol and mix well, heat to 60-80°C, stir at 180-240 rpm and 200-300 W / m 2 UV irradiation, reaction for 3.5-5h, after the reaction, centrifugation, washing and drying the lignin precipitate to obtain modified lignin;

[0016] Furthermore, the dosage ratio of fluorosilicified lignin, mercaptoethanol, benzoin dimethyl ether and dimethylacetamide is 50g:35-45mmol:8-12mg:60-70mL. Under light initiation, mercaptoethanol clicks with the unsaturated double bonds grafted on the fluorosilicified lignin to introduce active hydroxyl groups into the fluorosilicified lignin.

[0017] Beneficial effects of the present invention:

[0018] The present invention discloses an artificial board with a vertical and horizontal structure. A rotary cutting process is adopted along the growth direction of log fibers to obtain slices with oriented wood fibers. The slices are made into square materials with good processability by longitudinal lamination and gluing. The slices are longitudinally slicing and rotated to make the wood fibers crisscross to form an interwoven wood fiber network in space. When subjected to external force, the force is evenly dispersed, so that the board has higher mechanical strength and structural stability. In tests, the rigidity and warping resistance of the board are significantly improved.

[0019] The invention discloses a lignin adhesive suitable for an artificial balance board. The adhesive uses a traditional PMDI prepolymer as a bonding matrix and introduces a modified lignin independently developed to improve the water resistance of the adhesive layer. The adhesive is prepared by reacting highly active methylvinyldichlorosilane with hydroxyl groups on lignin molecules and tetrafluorobutanediol to introduce fluorine silicon structures and unsaturated double bonds into the lignin molecules. Then, mercaptoethanol and unsaturated double bonds grafted onto fluorosilicified lignin are click-reacted to introduce active hydroxyl groups into the fluorosilicified lignin. During the curing process of the adhesive, the active hydroxyl groups in the modified lignin can be effectively cross-linked with the PMDI prepolymer. Meanwhile, the thioether structure introduced by mercaptothiol and the oxygen and nitrogen structures in the curing chain form a chelating effect, and the chelating reinforcement is formed with the metal oxide filler to compensate for the problem of decreased bonding due to the fluorosilicified lignin. Thus, the adhesive maintains excellent bonding performance and has good waterproofness. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1, preparation of vertical and horizontal wood fiber balanced artificial board, the specific implementation process is as follows:

[0022] (1) Preparation of lignin adhesive

[0023] 1.1. Preparation of modified lignin

[0024] Step A1: Take lignin, tetrafluorobutanediol and anhydrous dioxane and add them into the mixture and ultrasonically disperse them for 10 minutes. Then, introduce dry nitrogen for protection, heat to 95°C, stir at 120 rpm, take equal amounts of methylvinyldichlorosilane and divide them into four parts, add them intermittently for 30 minutes, continue to stir and react at a constant temperature after the addition is complete, and control the total reaction time of methylvinyldichlorosilane to be 5 hours. The amount ratio of lignin, tetrafluorobutanediol, methylvinyldichlorosilane and anhydrous dioxane is 50 g: 20 mmol: 40 mmol: 100 mL. After the reaction is completed, remove dioxane by rotary evaporation to obtain fluorinated lignin.

[0025] Step A2: Premix fluorosilicified lignin, benzoin dimethyl ether and dimethylacetamide by ultrasonic for 10 min, pass nitrogen gas for protection, add mercaptoethanol and mix well, heat to 80°C, stir at 240 rpm and 300 W / m 2The reaction was carried out under ultraviolet irradiation for 3.5 hours, wherein the amount ratio of fluorosilicified lignin, mercaptoethanol, benzoin dimethyl ether and dimethylacetamide was 50 g:45 mmol:8 mg:70 mL. After the reaction was completed, the lignin precipitate layer was centrifuged, washed with water and dried to obtain modified lignin.

[0026] 1.2. Glue preparation

[0027] The raw materials are taken by weight: 100 parts of PMDI prepolymer, Lupranate WBP type raw material is used in the implementation process, -NCO content is 31.2%; 18 parts of modified lignin, prepared by this embodiment; 5 parts of metal oxide filler, 500 mesh zinc oxide powder is used in the implementation process; 0.4 parts of leveling agent, KMT-5502 type silicone leveling agent is used in the implementation process; 10 parts of diluent, industrial grade ethyl acetate is used in the implementation process;

[0028] The PMDI prepolymer, the leveling agent and the diluent were premixed at 120 rpm for 30 minutes, and then the modified lignin and the metal oxide filler were uniformly added and mixed at 30 rpm for 10 minutes to obtain a lignin adhesive.

[0029] (2) Preparation of vertical and horizontal wood fiber balanced artificial board

[0030] Step S1: Peel the log and dry the slices, control the moisture content of the slices to 12%, apply lignin adhesive on the surface, stack the slices longitudinally after coating, apply a pressure of 1.5 MPa perpendicular to the stacking direction, and cure at 80°C for 5 minutes to obtain square materials.

[0031] Step S2: Plane the square material longitudinally to form blanks, rotate adjacent blanks longitudinally, control the rotation angle to 90°, apply lignin adhesive to the planed surface of the blanks, stack them horizontally after gluing, apply 2MPa pressure perpendicular to the stacking direction, and cure at 100°C for 15 minutes to obtain a vertical and horizontal wood fiber balanced artificial board.

[0032] Example 2, preparation of vertical and horizontal wood fiber balanced artificial board, the specific implementation process is as follows:

[0033] (1) Preparation of lignin adhesive

[0034] 1.1. Preparation of modified lignin

[0035] Step A1: Take lignin, tetrafluorobutanediol and anhydrous dioxane and add them into the mixture and ultrasonically disperse them for 10 minutes. Then, introduce dry nitrogen for protection, heat the mixture to 85°C, stir at 90 rpm, take equal amounts of methylvinyldichlorosilane and divide them into four portions, add them intermittently for 30 minutes, continue to stir the reaction at a constant temperature after the addition is complete, and control the total reaction time of methylvinyldichlorosilane to be 7 hours. The amount ratio of lignin, tetrafluorobutanediol, methylvinyldichlorosilane and anhydrous dioxane is 50 g: 15 mmol: 30 mmol: 80 mL. After the reaction is completed, remove the dioxane by rotary evaporation to obtain fluorinated lignin.

[0036] Step A2: Premix fluorosilicified lignin, benzoin dimethyl ether and dimethylacetamide by ultrasonic for 10 min, pass nitrogen gas for protection, add mercaptoethanol and mix well, heat to 60°C, stir at 180 rpm and 200 W / m 2 The reaction was carried out under ultraviolet irradiation for 5 hours, wherein the amount ratio of fluorosilicified lignin, mercaptoethanol, benzoin dimethyl ether and dimethylacetamide was 50 g: 35 mmol: 12 mg: 60 mL. After the reaction was completed, the lignin precipitate layer was centrifuged, washed with water and dried to obtain modified lignin.

[0037] 1.2. Glue preparation

[0038] The raw materials are taken by weight: 100 parts of PMDI prepolymer, Lupranate WBP type raw material is used in the implementation process, -NCO content is 31.2%; 26 parts of modified lignin, prepared by this embodiment; 8 parts of metal oxide filler, 500 mesh zinc oxide powder is used in the implementation process; 0.5 parts of leveling agent, KMT-5502 type silicone leveling agent is used in the implementation process; 15 parts of diluent, industrial grade ethyl acetate is used in the implementation process;

[0039] The PMDI prepolymer, the leveling agent and the diluent were premixed at 120 rpm for 30 minutes, and then the modified lignin and the metal oxide filler were uniformly added and mixed at 30 rpm for 10 minutes to obtain a lignin adhesive.

[0040] (2) Preparation of vertical and horizontal wood fiber balanced artificial board

[0041] Step S1: Peel the log and dry the slices, control the moisture content of the slices to 12%, apply lignin adhesive on the surface, stack the slices longitudinally after coating, apply a pressure of 1.5 MPa perpendicular to the stacking direction, and cure at 80°C for 5 minutes to obtain square materials.

[0042] Step S2: Plane the square material longitudinally to form blanks, rotate adjacent blanks longitudinally, control the rotation angle to 90°, apply lignin adhesive to the planed surface of the blanks, stack them horizontally after gluing, apply 2MPa pressure perpendicular to the stacking direction, and cure at 100°C for 15 minutes to obtain a vertical and horizontal wood fiber balanced artificial board.

[0043] Example 3, preparation of vertical and horizontal wood fiber balanced artificial board, the specific implementation process is as follows:

[0044] (1) Preparation of lignin adhesive

[0045] 1.1. Preparation of modified lignin

[0046] Step A1: Take lignin, tetrafluorobutanediol and anhydrous dioxane and add them into the mixture and ultrasonically disperse them for 10 minutes. Then, introduce dry nitrogen for protection, heat the mixture to 90°C, stir the mixture at 90 rpm, take equal amounts of methylvinyldichlorosilane and divide them into four portions, add them intermittently for 30 minutes, continue to stir the mixture at a constant temperature after the addition is complete, and control the total reaction time of methylvinyldichlorosilane to be 6 hours. The amount ratio of lignin, tetrafluorobutanediol, methylvinyldichlorosilane and anhydrous dioxane is 50 g: 18 mmol: 35 mmol: 90 mL. After the reaction is completed, dioxane is removed by rotary evaporation to obtain fluorinated lignin.

[0047] Step A2: Premix fluorosilicified lignin, benzoin dimethyl ether and dimethylacetamide by ultrasonic for 10 min, pass nitrogen protection, add mercaptoethanol and mix well, heat to 70 °C, stir at 180 rpm and 260 W / m 2 The reaction was carried out under ultraviolet irradiation for 4 hours, wherein the amount ratio of fluorosilicified lignin, mercaptoethanol, benzoin dimethyl ether and dimethylacetamide was 50 g: 40 mmol: 10 mg: 65 mL. After the reaction was completed, the lignin precipitate layer was centrifuged, washed with water and dried to obtain modified lignin.

[0048] 1.2. Glue preparation

[0049] The raw materials are taken by weight: 100 parts of PMDI prepolymer, Lupranate WBP type raw material is used in the implementation process, -NCO content is 31.2%; 20 parts of modified lignin, prepared by this embodiment; 7 parts of metal oxide filler, 500 mesh alumina and titanium oxide micropowder are used in the implementation process according to the mass ratio of 2:1; 0.4 parts of leveling agent, KMT-5502 type silicone leveling agent is used in the implementation process; 12 parts of diluent, industrial grade ethyl acetate is used in the implementation process;

[0050] The PMDI prepolymer, the leveling agent and the diluent were premixed at 120 rpm for 30 minutes, and then the modified lignin and the metal oxide filler were uniformly added and mixed at 30 rpm for 10 minutes to obtain a lignin adhesive.

[0051] (2) Preparation of vertical and horizontal wood fiber balanced artificial board

[0052] Step S1: Peel the log and dry the slices, control the moisture content of the slices to 12%, apply lignin adhesive on the surface, stack the slices longitudinally after coating, apply a pressure of 1.5 MPa perpendicular to the stacking direction, and cure at 80°C for 5 minutes to obtain square materials.

[0053] Step S2: Plane the square material longitudinally to form blanks, rotate adjacent blanks longitudinally, control the rotation angle to 90°, apply lignin adhesive to the planed surface of the blanks, stack them horizontally after gluing, apply 2MPa pressure perpendicular to the stacking direction, and cure at 100°C for 15 minutes to obtain a vertical and horizontal wood fiber balanced artificial board.

[0054] Example 4, preparation of vertical and horizontal wood fiber balanced artificial board, the specific implementation process is as follows:

[0055] (1) Preparation of lignin adhesive

[0056] 1.1. Preparation of modified lignin

[0057] Step A1: Take lignin, tetrafluorobutanediol and anhydrous dioxane and add them into the mixture and ultrasonically disperse them for 10 minutes. Then, introduce dry nitrogen for protection, heat to 90°C, stir at 120 rpm, take equal amounts of methylvinyldichlorosilane and divide them into four parts, add them intermittently for 30 minutes, continue to stir and react at a constant temperature after the addition is complete, and control the total reaction time of methylvinyldichlorosilane to be 6.5 hours. The amount ratio of lignin, tetrafluorobutanediol, methylvinyldichlorosilane and anhydrous dioxane is 50 g: 20 mmol: 35 mmol: 90 mL. After the reaction is completed, dioxane is removed by rotary evaporation to obtain fluorinated lignin.

[0058] Step A2: Premix fluorosilicified lignin, benzoin dimethyl ether and dimethylacetamide by ultrasonic for 10 min, pass nitrogen gas for protection, add mercaptoethanol and mix well, heat to 65 °C, stir at 240 rpm and 220 W / m 2 The reaction was carried out under ultraviolet irradiation for 4.5 hours, wherein the amount ratio of fluorosilicified lignin, mercaptoethanol, benzoin dimethyl ether and dimethylacetamide was 50 g: 40 mmol: 12 mg: 70 mL. After the reaction was completed, the lignin precipitate was centrifuged, washed with water and dried to obtain modified lignin.

[0059] 1.2. Glue preparation

[0060] The raw materials are taken by weight: 100 parts of PMDI prepolymer, Lupranate WBP type raw material is used in the implementation process, -NCO content is 31.2%; 23 parts of modified lignin, prepared by this embodiment; 6 parts of metal oxide filler, 500 mesh alumina and titanium oxide powder are compounded in a mass ratio of 2:1 in the implementation process; 0.5 parts of leveling agent, KMT-5502 type silicone leveling agent is used in the implementation process; 13 parts of diluent, industrial grade ethyl acetate is used in the implementation process;

[0061] The PMDI prepolymer, the leveling agent and the diluent were premixed at 120 rpm for 30 minutes, and then the modified lignin and the metal oxide filler were uniformly added and mixed at 30 rpm for 10 minutes to obtain a lignin adhesive.

[0062] (2) Preparation of vertical and horizontal wood fiber balanced artificial board

[0063] Step S1: Peel the log and dry the slices, control the moisture content of the slices to 12%, apply lignin adhesive on the surface, stack the slices longitudinally after coating, apply a pressure of 1.5 MPa perpendicular to the stacking direction, and cure at 80°C for 5 minutes to obtain square materials.

[0064] Step S2: Plane the square material longitudinally to form blanks, rotate adjacent blanks longitudinally, control the rotation angle to 90°, apply lignin adhesive to the planed surface of the blanks, stack them horizontally after gluing, apply 2MPa pressure perpendicular to the stacking direction, and cure at 100°C for 15 minutes to obtain a vertical and horizontal wood fiber balanced artificial board.

[0065] Comparative Example 1

[0066] This comparative example is a commercially available multi-layer solid wood balance board.

[0067] Comparative Example 2

[0068] This comparative example refers to Example 4, except that the modified lignin is replaced by the lignin raw material, and the rest of the implementation process is exactly the same.

[0069] Take the above balance board and test the stiffness of the balance board according to the ASTM D1037-12 standard; test the warpage of the balance board according to the ISO 23999-2021 standard, test the heat resistance warpage by baking at 70°C for 3 hours, and test the water resistance warpage by immersing in water at room temperature for 24 hours; test the water absorption thickness expansion rate of the balance board according to the NALFA LF01 standard; the specific test results are shown in the following table:

[0070] Stiffness / N Heat resistance warpage / % Water resistance warping / % Thickness expansion rate / % Example 1 379.2 0.19 0.16 0.29 Example 2 415.5 0.12 0.11 0.35 Example 3 391.0 0.15 0.14 0.25 Example 4 402.9 0.11 0.08 0.21 Comparative Example 1 286.4 0.69 0.53 1.27 Comparative Example 2 337.5 0.31 0.38 1.08

[0071] It can be seen from the test results in the above table that the balance board of the embodiment has higher rigidity, is resistant to heat warping, water warping and water expansion, and has excellent structural stability.

[0072] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0073] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A production process for vertical and horizontal wood fiber balanced artificial board, characterized in that: Including the following processes: Step S1: the log is peeled and the slices are dried, and then lignin adhesive is applied in sequence, the slices are longitudinally stacked and pressurized to obtain square materials; Step S2: Plane the square material longitudinally to form green sheets, rotate adjacent green sheets longitudinally, and then sequentially coat the green sheets with lignin adhesive, transversely stack and press-cure to obtain vertical and horizontal wood fiber balanced artificial boards.

2. The production process of a vertical and horizontal wood fiber balanced artificial board according to claim 1 is characterized in that: The lignin adhesive comprises, by weight: 100 parts of PMDI prepolymer, 18-26 parts of modified lignin, 5-8 parts of metal oxide filler, 0.4-0.5 parts of leveling agent and 10-15 parts of diluent; The modified lignin is prepared by the following method: Step A1: ultrasonically disperse lignin, tetrafluorobutanediol and anhydrous dioxane, introduce dry nitrogen for protection, heat to 85-95°C, stir at 90-120 rpm, intermittently add methylvinyldichlorosilane to react for 5-7 hours, and remove dioxane by rotary evaporation after the reaction to obtain fluorosilicified lignin; Step A2: Premix fluorosilicified lignin, benzoin dimethyl ether and dimethylacetamide by ultrasonication, pass nitrogen protection, add mercaptoethanol and mix well, heat to 60-80°C, stir at 180-240 rpm and 200-300 W / m 2 The reaction was carried out under ultraviolet irradiation for 3.5-5 hours. After the reaction was completed, the lignin precipitate was centrifuged and washed with water and dried to obtain modified lignin.

3. The production process of a vertical and horizontal wood fiber balanced artificial board according to claim 2 is characterized in that: The usage ratio of lignin, tetrafluorobutanediol, methylvinyldichlorosilane and anhydrous dioxane is 50g:15-20mmol:30-40mmol:80-100mL.

4. The production process of a vertical and horizontal wood fiber balanced artificial board according to claim 3 is characterized in that: The usage ratio of fluorosilicified lignin, mercaptoethanol, benzoin dimethyl ether and dimethylacetamide is 50g:35-45mmol:8-12mg:60-70mL.

5. The production process of a vertical and horizontal wood fiber balanced artificial board according to claim 2, characterized in that: The -NCO content of PMDI prepolymer is 30-35%.

6. The production process of a vertical and horizontal wood fiber balanced artificial board according to claim 2 is characterized in that: The metal oxide filler is one or more of zinc oxide, titanium oxide and aluminum oxide.

7. The production process of a vertical and horizontal wood fiber balanced artificial board according to claim 1 is characterized in that: The vertical rotation angle is 90°.

8. A vertical and horizontal wood fiber balanced artificial board, characterized in that: Made by the production process described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Floor and its production method and its uses as ground heat floor

    CN101054852A

  • Waterproof lignin-based epoxy resin adhesive and preparation method thereof

    CN112126391A

  • Formaldehyde-free flame-retardant lignin adhesive and preparation method thereof

    CN118085814A