Flanged large-diameter lining-free composite material pipeline for liquid oxygen environment and preparation method of flange large-diameter lining-free composite material pipeline
By adopting a multi-layer structure design of carbon fiber composite materials and specially made composite epoxy resin, the problems of anti-seepage and pressure tolerance of composite flanges in liquid oxygen environment are solved, and weight reduction and liquid oxygen compatibility are improved to ensure that The sealing and mechanical properties of composite pipes are provided.
Patent Information
- Application Number
- CN202411201534.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
Existing composite flanges have challenges in anti-seepage and pressure resistance in liquid oxygen environments, and traditional metal materials do not meet the needs of lightweighting.
Carbon fiber composite materials are used to replace traditional metal materials, and through the optimization of flange structure design and impregnation technology of specially made composite epoxy resin, a multi-layer composite pipeline is formed, including anti-seepage layer, transition layer and reinforcement layer, combined with nanofillers and specific resin systems to improve liquid oxygen compatibility and sealing properties.
It realizes significant weight reduction without sacrificing structural strength and sealing properties, and at the same time improves anti-permeability and liquid oxygen compatibility under low-temperature environments, ensuring good wetting and bonding between fibers and resins, and is equipped with Excellent sealing performance and liquid oxygen compatibility.
Smart Images

Figure CN119042422A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a large-diameter, non-lined composite material pipeline with a flange for use in a liquid oxygen environment and a preparation method thereof, and belongs to the technical field of resin-based composite materials. Background Art
[0002] With the advancement of aerospace technology, the requirements for rocket boosters are also increasing, and efficient and environmentally friendly liquid oxygen fuel is being used in rocket boosters. However, since the composite flange is installed at the manhole of the liquid oxygen tank and liquid oxygen has low temperature characteristics, this puts a test on the low temperature anti-seepage ability and pressure bearing capacity of the composite material.
[0003] At the same time, in the composite material molding process, fiber winding is an important processing technology with a long history and wide application, especially in the aerospace field such as fuel tanks, aircraft auxiliary fuel tanks, and the civilian market of pressure vessels such as pressure pipes, storage tanks, and gas cylinders. The fiber winding process has the advantages of high precision, high production efficiency and low labor intensity. The fiber winding molding process is usually divided into three types: dry winding, wet winding and semi-dry winding. Among them, wet winding is the most widely used method because it has many advantages such as low cost, wide application field, little damage to fibers and long material storage period, which is significantly better than the other two methods. However, wet winding requires the use of resin systems. These resins must have good fiber wettability and adhesion, and have high strength and elongation suitable for the fibers after curing.
[0004] In order to meet the requirements of composite flange structure and pipeline, the resin itself must have good liquid oxygen compatibility, and can resist the expansion of combustion reaction when stimulated by ignition sources such as impact, friction, vibration, etc. in liquid oxygen environment without combustion reaction. The existing resin system is generally tested at 98J energy. If no reaction occurs in the first 20 tests, it proves that the material is compatible with liquid oxygen.
[0005] Chinese patent application CN111137472A - The upper surface of the inner annular flange in a large-diameter unlined composite tank connection structure is set as a curved surface to ensure that there is no obvious transition on the winding surface, and the safety and sealing performance of the tank structure after winding are improved. However, its flange structure is still made of metal material and does not meet the lightweight requirements. Chinese patent application CN116515247A - A method for preparing an epoxy resin system and a composite material for a liquid oxygen tank, in which phosphorus-containing epoxy resin is added, can finally meet the basic liquid oxygen compatibility test requirements, but cannot achieve high liquid oxygen compatibility. Summary of the invention
[0006] In order to solve the above problems, the present application proposes a large-diameter, unlined composite pipeline with flange for liquid oxygen environment and a preparation method thereof. By adopting carbon fiber composite materials instead of traditional metal materials and optimizing the flange structure design, it is possible to achieve a significant weight reduction without sacrificing structural strength and sealing. At the same time, it is impregnated with a special composite epoxy resin to improve the anti-penetration ability of the pipeline in the low-temperature environment of liquid oxygen, ensure better wetting and bonding between the fiber and the resin, and have excellent sealing performance and liquid oxygen compatibility.
[0007] According to one aspect of the present application, there is provided a large-diameter, unlined composite pipeline with flange for use in a liquid oxygen environment, comprising a connecting section and a pipeline section;
[0008] The connecting section comprises a flange layer and a sealing groove, wherein the flange layer is made of a carbon fiber woven cloth layer impregnated with a composite epoxy resin, and the sealing groove is arranged on the end face of the flange layer for end face sealing;
[0009] The pipeline section includes an impermeable layer, a transition layer and a reinforcement layer from the inside to the outside. The impermeable layer is obtained by curing the carbon fiber surface felt impregnated with a composite epoxy resin; the transition layer is formed by winding a carbon fiber woven cloth; the reinforcement layer is made by combining a carbon fiber woven cloth impregnated with a composite epoxy resin and a carbon fiber yarn through laying and winding.
[0010] This application adopts a multi-layer structure design of the pipeline section:
[0011] The anti-seepage layer is obtained by impregnating the carbon fiber surface felt with composite epoxy resin and then curing it. The carbon fiber surface felt has good adsorption capacity and uniform fiber distribution, and can evenly adsorb and cure epoxy resin to form a dense anti-seepage layer. It can effectively prevent the penetration of liquid oxygen and ensure the anti-seepage effect of the pipeline in the low temperature environment of liquid oxygen.
[0012] The transition layer is formed by winding carbon fiber woven cloth. Through circumferential winding, the structural stability and pressure resistance of the pipeline can be improved. As the intermediate layer between the anti-seepage layer and the reinforcement layer, the transition layer plays a good transition and buffering role, and enhances the stability of the overall structure.
[0013] The reinforcement layer is made of multiple layers of carbon fiber woven cloth and yarn laid and wound together, and has high strength, high modulus and excellent impact resistance. It can maintain good mechanical properties in liquid oxygen low temperature environment and high pressure environment, ensuring the long-term service life of the pipeline.
[0014] At the same time, only resin-impregnated carbon fiber cloth layers are used in the anti-seepage layer, reinforcement layer and flange layer, and ordinary carbon fiber cloth is used in the transition layer. This can not only ensure good bonding between the layers, stable interface and smooth transition, but also ensure that the middle transition layer has a certain flexibility, so that the hardness difference between the anti-seepage layer and the reinforcement layer is effectively buffered, avoiding poor interlayer bonding caused by hardness difference.
[0015] Optionally, the anti-seepage layer has a glue content of 45-55% after dipping, and the reinforcement layer and the flange layer have a glue content of 25-35% after dipping;
[0016] The transition layer is formed by hoop-winding two layers of carbon fiber woven fabric.
[0017] Specifically, by limiting the amount of glue in the anti-seepage layer, the carbon fiber surface felt can be fully impregnated with epoxy resin, filling the pores between the fibers to form a dense anti-seepage layer, which can effectively prevent the penetration of liquid oxygen and ensure the anti-seepage effect. At the same time, the amount of glue can ensure that the resin is evenly distributed on the carbon fiber surface felt to form a uniform and consistent anti-seepage layer, avoiding the problem of uneven anti-seepage performance caused by local excessive thickness or thinness.
[0018] By limiting the amount of glue in the reinforcement layer and flange layer, the carbon fiber woven cloth and yarn can be evenly impregnated with epoxy resin to form a reinforcement layer and flange layer with high strength and high modulus. This amount of glue can improve the interlayer bonding force, thereby enhancing the mechanical properties of the overall structure. At the same time, this amount of glue can ensure uniform distribution of the resin, avoid problems such as interlayer delamination and cracks caused by excessive or insufficient resin content, and improve structural stability and durability.
[0019] Optionally, the composite epoxy resin is prepared from the following raw materials, measured in parts by weight: 80-100 parts of compound epoxy resin, 5-10 parts of composite nanofiller, 10-20 parts of ether diluent, 5-15 parts of flame retardant and 30-50 parts of amine curing agent; the compound epoxy resin includes bromine-containing epoxy resin, and the composite nanofiller includes at least two silane-modified nanomaterials.
[0020] Optionally, the compounded epoxy resin further comprises polyimide and m-phenylenediamine; the weight ratio of the bromine-containing epoxy resin to the polyimide is (2-4):1, and the amount of m-phenylenediamine used is 2-5% of the epoxy equivalent of the bromine-containing epoxy resin;
[0021] The bromine-containing epoxy resin includes brominated bisphenol A epoxy resin or brominated bisphenol F epoxy resin.
[0022] Specifically, bromine-containing epoxy resin is preferred because it has good antioxidant and flame retardant properties, helps resist combustion reactions in liquid oxygen environments, and improves the safety and stability of the material. It is then modified using polyimide and meta-phenylenediamine, whereby the imide group reacts with the epoxy group to undergo an addition reaction and chemical crosslinking occurs, thereby improving the liquid oxygen compatibility of the resin system. Polyimide provides tough segments to improve resistance to liquid oxygen impact, and meta-phenylenediamine acts as an auxiliary curing agent to promote co-curing reactions and increase the degree of crosslinking. The two help to comprehensively improve the performance of bromine-containing epoxy resin.
[0023] Optionally, the composite nanofiller includes modified boron nitride nanotubes and modified alumina nanosheets in a weight ratio of 1:(2-5).
[0024] Preferably, the outer diameter of the boron nitride nanotubes is in the range of 30-80 nm, and the axial ratio (length / diameter) is between 10-30; the size range of the aluminum oxide nanosheets is 2-5 nm in thickness and 80-100 nm in side length.
[0025] Optionally, the modification method of the boron nitride nanotubes and aluminum oxide nanosheets is: pre-treating the surfaces of the boron nitride nanotubes and aluminum oxide nanosheets with dilute hydrochloric acid, adding a silane coupling agent KH-550 ethanol solution, ultrasonically treating, washing and drying.
[0026] Specifically, 2% by mass of dilute hydrochloric acid and 5% of KH-550 ethanol solution are used, and the boron nitride nanotubes and aluminum oxide nanosheets are first impregnated with dilute hydrochloric acid for 0.5 h, and then added into the KH-550 ethanol solution after pretreatment, and then ultrasonically treated for 0.5 h after mixing evenly, reacted at 70° C. for 1 h, and washed and dried after the reaction.
[0027] Boron nitride nanotubes can be used to improve liquid oxygen compatibility. The one-dimensional nanostructure with high axial ratio can produce a variety of crack deflections, which plays a toughening role. At the same time, they contain BN bonds and have good oxidation resistance, which can inhibit the oxidative degradation of epoxy resin in liquid oxygen environment. Alumina nanosheets are also used. Their plate-like two-dimensional structure can produce interlayer shear effects to enhance the mechanical properties of the resin. At the same time, the high specific surface area can improve the interfacial bonding force and enhance the liquid oxygen compatibility. The synergistic effect of the two different dimensional structures improves the tolerance level of liquid oxygen impact energy.
[0028] Furthermore, by modifying the two nanofillers with silane, the bonding strength between the inorganic filler and the organic resin interface was significantly improved, and the ability of the resin to withstand liquid oxygen shock was enhanced. After obtaining uniform and stable modified nanofillers by ultrasonic dispersion, and then mixing and curing with the resin, the dispersion of the fillers can be effectively improved and the impact toughness of the resin can be enhanced.
[0029] Optionally, the flame retardant is a phosphoric acid acrylate monomer containing a double bond.
[0030] Specifically, by using double-bond phosphate acrylate monomers, the double bonds react with the epoxy resin to chemically anchor the flame retardant groups stably on the resin network, thereby effectively improving the flame retardant properties of the epoxy resin.
[0031] Optionally, the amine curing agent is one of m-phenylenediamine and 4,4'-diaminodiphenyl ether.
[0032] Optionally, the ether diluent includes one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, phenyl glycidyl ether and 4-tert-butylphenyl glycidyl ether.
[0033] Specifically, the preparation method of the compound epoxy resin comprises the following steps:
[0034] (1) adding a flame retardant to the compounded epoxy resin and mixing them evenly to carry out a modification reaction;
[0035] (2) Add the composite nano-filler and the ether diluent, stir and disperse, and then add the amine curing agent and stir evenly to obtain the product.
[0036] Optionally, the compounded epoxy resin in step (1) is obtained by pre-reacting a mixture of bromine-containing epoxy resin, polyimide and meta-phenylenediamine, the pre-reaction temperature is 60-80°C, and the reaction time is 1-2h; the reaction temperature in step (1) is 50-60°C and the reaction time is 1-2h.
[0037] Specifically, the stirring rate in step (2) is 600-1000 rpm, and the time is 2-4 h.
[0038] According to another aspect of the present application, a method for preparing the composite material pipeline is provided, comprising the following steps:
[0039] (1) Install the core mold on the winding machine, spray the release agent on the surface of the core mold, and leave it for 5-10 hours after spraying;
[0040] (2) The carbon fiber surface felt is impregnated with a compound epoxy resin and then pre-cured. After the pre-curing is completed, the carbon fiber surface felt is taken out and laid flat on the surface of the core mold, and rolled into a cylinder as the mold rotates to form an impermeable layer;
[0041] (3) After the pre-curing of the anti-seepage layer is completed, two layers of carbon fiber woven fabrics are sequentially fastened on the outer surface of the anti-seepage layer by a circumferential winding method to form a transition layer;
[0042] (4) Continue to lay the composite epoxy resin impregnated carbon fiber woven cloth by circumferential fiber laying and winding to lay several reinforcement layers and flange layers. After the winding is completed, vacuum the pipeline and perform high-temperature curing to finally form the composite material pipeline.
[0043] Optionally, in step (2), the pre-curing temperature is 50-90° C., and the pre-curing time is 1.5-2 h;
[0044] Step (4) also includes:
[0045] a. First lay a layer of carbon fiber woven cloth with straight flange impregnated with composite epoxy resin, and then lay the reinforcement layer in the circumferential direction;
[0046] b. The number of reinforcement layers is 5-8 in total. After each reinforcement layer is laid, 15-25 layers of carbon fiber woven cloth impregnated with composite epoxy resin need to be laid to gradually form the flange layer;
[0047] c. Repeat steps a and b 3-4 times, cutting off the excess part at the edge of the flange each time to finally form a flange layer.
[0048] Preferably, in step a, after laying 3-5 layers of reinforcement layers, the flange is compacted by hammering with a rubber hammer;
[0049] In step b, 15 layers of carbon fiber woven fabric impregnated with composite epoxy resin are laid, and the layers need to be staggered at the seams during the laying process;
[0050] In addition, in step (4), after winding is completed but before vacuum high-temperature curing, the excess glue needs to be scraped out in a circumferential direction.
[0051] Specifically, in step (4), the vacuum degree is 0.1-0.3 mbar, and the high temperature curing is firstly to uniformly heat from 30°C to 90°C within 60 minutes, and keep warm for 2-3 hours; then to uniformly heat to 120°C within 60 minutes, and keep warm for 2-4 hours; finally to uniformly heat to 160°C within 60 minutes, and keep warm for 2-4 hours.
[0052] Specifically, after winding to form a transition layer, composite resin is used to bond the interface, and the release agent is commercially available polytetrafluoroethylene wax. The sealing groove is machined on the flange end face after high temperature curing to form a sealing groove for end face sealing, such as a conventional annular groove.
[0053] The beneficial effects of this application include but are not limited to:
[0054] 1. The composite material pipeline provided in this application can achieve a significant reduction in weight without sacrificing structural strength and sealing by adopting specific composite materials and winding processing methods; at the same time, it is impregnated with a special composite epoxy resin to improve the pipeline's anti-penetration ability in a liquid oxygen low-temperature environment, ensure better wetting and bonding between the fiber and the resin, and have excellent sealing performance and liquid oxygen compatibility.
[0055] 2. The composite material pipeline provided in the present application has a large number of micro-fluffs on the surface of the carbon fiber felt through structural optimization combined with a gradient design of the glue content. Combined with the composite epoxy resin with a moderate glue content, a tight fiber structure is provided to form a dense anti-seepage layer, which maintains good chemical stability and mechanical strength at low temperatures, thereby preventing liquid oxygen penetration. At the same time, two layers of carbon fiber woven cloth are circumferentially wound to form a transition layer, which not only improves the sealing effect, but also avoids the damage of the anti-seepage layer to produce gaps due to direct fiber winding and tightening, and further limits the low glue content of the reinforcement layer to ensure the maximum load transfer of the fiber, while the uniform distribution of the epoxy resin provides good crack resistance and impact resistance.
[0056] 3. The composite material pipeline provided in the present application adopts a basic resin system formed by co-curing a bromine-containing epoxy resin and polyimide, thereby improving the compatibility with liquid oxygen while taking into account the mechanical properties. The polyimide resin segment provides good toughness and enhances the ability of the resin to resist liquid oxygen impact.
[0057] 4. The preparation method of the composite material pipeline provided in the present application first pre-cures the anti-seepage layer so that the resin in the carbon fiber surface felt reaches a "semi-cured" state, that is, the resin becomes strong enough to maintain its shape and structure, but still retains a certain flexibility and viscosity. The pre-cured resin state ensures that when the carbon fiber woven cloth of the transition layer is applied thereto, it can achieve a tight fit without gaps, ensuring the transfer of mechanical properties and chemical stability between layers, and more importantly, preventing liquid penetration and stress concentration.
[0058] 5. The method for preparing the composite material pipeline provided in the present application adopts cross-laying and limits the number of laying layers, and performs specific treatment on the right-angle section of the flange, thereby increasing the bearing capacity of the flange, helping to better distribute the stress generated at the connection, avoiding stress concentration, and thus improving the reliability of the connection. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0060] Figure 1 This is a schematic diagram of the cross-sectional structure of a large-diameter, unlined composite material pipeline with a flange for liquid oxygen environment involved in Example 1 of the present application.
[0061] Reference numerals: 1. flange layer; 2. anti-seepage layer; 3. transition layer; 4. reinforcement layer. DETAILED DESCRIPTION
[0062] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0063] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in this patent are for demonstration purposes only.
[0064] Example 1
[0065] A large-diameter, unlined composite pipeline with flange for liquid oxygen environment comprises a connecting section and a pipeline section; the connecting section comprises a flange layer 1 and a sealing groove, the flange layer 1 is made of a carbon fiber woven cloth impregnated with a compound epoxy resin, and the sealing groove is arranged on the end face of the flange layer 1 for end face sealing; the pipeline section comprises an impermeable layer 2, a transition layer 3 and a reinforcing layer 4 from the inside to the outside, the impermeable layer 2 is obtained by curing the carbon fiber surface felt impregnated with a compound epoxy resin; the transition layer 3 is formed by winding a carbon fiber woven cloth; the reinforcing layer 4 is made by combining a carbon fiber woven cloth impregnated with a compound epoxy resin and a carbon fiber yarn through laying and winding.
[0066] The rubber content of the impregnated layer 2 is 50%, and the rubber content of the reinforcing layer 4 and the flange layer 1 is 30% after being impregnated; the transition layer 3 is formed by circumferentially winding two layers of carbon fiber woven cloth.
[0067] The composite epoxy resin is prepared from the following raw materials in parts by weight: 90 parts of compound epoxy resin, 7 parts of composite nano filler, 15 parts of ether diluent, 10 parts of flame retardant and 40 parts of amine curing agent.
[0068] The compound epoxy resin also includes polyimide and metaphenylenediamine; the weight ratio of the bromine-containing epoxy resin to the polyimide is 3:1, and the amount of metaphenylenediamine is 4% of the epoxy equivalent of the bromine-containing epoxy resin; the bromine-containing epoxy resin is brominated bisphenol A epoxy resin. The composite nanofiller includes modified boron nitride nanotubes and modified alumina nanosheets, with a weight ratio of 1:4.
[0069] The modification method of boron nitride nanotubes and aluminum oxide nanosheets is as follows: using 2% by mass dilute hydrochloric acid and 5% KH-550 ethanol solution, the boron nitride nanotubes and aluminum oxide nanosheets are first immersed in dilute hydrochloric acid for 0.5 h, and after pretreatment, they are added into the KH-550 ethanol solution respectively, mixed evenly and then ultrasonically treated for 0.5 h, reacted at 70° C. for 1 h, and washed and dried after the reaction.
[0070] The flame retardant is a phosphoric acid acrylate monomer containing a double bond, the amine curing agent is m-phenylenediamine, and the ether diluent is ethylene glycol dimethyl ether.
[0071] The preparation method comprises the following steps:
[0072] (1) adding a flame retardant to the compounded epoxy resin and mixing them evenly to carry out a modification reaction;
[0073] (2) Add the composite nanofiller and ether diluent, stir and disperse, and then add the amine curing agent and stir evenly to obtain. The composite epoxy resin in step (1) is obtained by pre-reacting a mixture of bromine-containing epoxy resin, polyimide and m-phenylenediamine, the pre-reaction temperature is 80°C, and the reaction time is 1 hour; the reaction temperature in step (1) is 60°C and the reaction time is 1 hour. The stirring rate in step (2) is 800 rpm and the reaction time is 3 hours.
[0074] The method for preparing the composite material pipeline comprises the following steps:
[0075] (1) Install the core mold on the winding machine, spray the release agent on the surface of the core mold, and leave it for 6 hours after spraying;
[0076] (2) The carbon fiber surface felt is impregnated with a compound epoxy resin and then pre-cured. After the pre-curing is completed, the carbon fiber surface felt is taken out and laid flat on the surface of the core mold, and rolled into a cylinder as the mold rotates to form an impermeable layer 2;
[0077] (3) After the pre-curing of the anti-seepage layer 2 is completed, two layers of carbon fiber woven fabrics are sequentially fastened on the outer surface of the anti-seepage layer 2 by means of hoop winding to form a transition layer 3;
[0078] (4) Continue to lay the composite epoxy resin impregnated carbon fiber woven cloth by circumferential fiber laying and winding to lay several reinforcement layers 4 and flange layers 1. After the winding is completed, the pipeline is vacuumed and high-temperature cured by vacuuming to finally form a composite material pipeline.
[0079] Wherein, in step (2), the pre-curing temperature is 80°C and the pre-curing time is 2h;
[0080] Step (4) also includes:
[0081] a. First lay a layer of carbon fiber woven cloth with straight flange impregnated with composite epoxy resin, and then lay the reinforcement layer 4 in the circumferential direction;
[0082] b. The number of reinforcement layers 4 is 6 in total. After each reinforcement layer 4 is laid, 15 layers of carbon fiber woven cloth impregnated with composite epoxy resin need to be laid to gradually form flange layer 1;
[0083] c. Repeat steps a and b three times, cutting off the excess portion at the flange edge each time, and finally forming flange layer 1.
[0084] The vacuum degree of step (4) is 0.1-0.3 mbar, and the high temperature curing is firstly to uniformly heat from 30°C to 90°C within 60 minutes and keep it warm for 2 hours; then to uniformly heat to 120°C within 60 minutes and keep it warm for 3 hours; finally to uniformly heat to 160°C within 60 minutes and keep it warm for 3 hours.
[0085] Example 2
[0086] A large-diameter, unlined composite pipeline with flange for liquid oxygen environment comprises a connecting section and a pipeline section; the connecting section comprises a flange layer and a sealing groove, the flange layer is made of a carbon fiber woven cloth impregnated with a compound epoxy resin, and the sealing groove is arranged on the end face of the flange layer for end face sealing; the pipeline section comprises an impermeable layer, a transition layer and a reinforcing layer from the inside to the outside, the impermeable layer is obtained by curing the carbon fiber surface felt impregnated with a compound epoxy resin; the transition layer is formed by winding a carbon fiber woven cloth; the reinforcing layer is made by combining a carbon fiber woven cloth impregnated with a compound epoxy resin and a carbon fiber yarn through a laying and winding method.
[0087] The rubber content of the impregnated layer is 45%, and the rubber content of the reinforcing layer and the flange layer is 35% after being impregnated; the transition layer is formed by circumferentially winding two layers of carbon fiber woven cloth.
[0088] The composite epoxy resin is the same as that in Example 1.
[0089] The method for preparing the composite material pipeline comprises the following steps:
[0090] (1) Install the core mold on the winding machine, spray the release agent on the surface of the core mold, and leave it for 5 hours after spraying;
[0091] (2) The carbon fiber surface felt is impregnated with a compound epoxy resin and then pre-cured. After the pre-curing is completed, the carbon fiber surface felt is taken out and laid flat on the surface of the core mold, and rolled into a cylinder as the mold rotates to form an impermeable layer;
[0092] (3) After the pre-curing of the anti-seepage layer is completed, two layers of carbon fiber woven fabrics are sequentially fastened on the outer surface of the anti-seepage layer by a circumferential winding method to form a transition layer;
[0093] (4) Continue to lay the composite epoxy resin impregnated carbon fiber woven cloth by circumferential fiber laying and winding to lay several reinforcement layers and flange layers. After the winding is completed, the pipeline is vacuumed and high-temperature cured by vacuuming to finally form a composite material pipeline.
[0094] Wherein, in step (2), the pre-curing temperature is 50°C and the pre-curing time is 2h;
[0095] Step (4) also includes:
[0096] a. First lay a layer of carbon fiber woven cloth with straight flange impregnated with composite epoxy resin, and then lay the reinforcement layer in the circumferential direction;
[0097] b. There are 5 reinforcement layers in total. After each reinforcement layer is laid, 20 layers of carbon fiber woven cloth impregnated with composite epoxy resin need to be laid to gradually form the flange layer;
[0098] c. Repeat steps a and b 4 times, cutting off the excess part at the edge of the flange each time to finally form a flange layer.
[0099] The vacuum degree of step (4) is 0.1-0.3 mbar, and the high temperature curing is firstly to uniformly heat from 30°C to 90°C within 60 minutes, and keep it warm for 2 hours; then to uniformly heat to 120°C within 60 minutes, and keep it warm for 4 hours; finally to uniformly heat to 160°C within 60 minutes, and keep it warm for 4 hours.
[0100] Example 3
[0101] A large-diameter, unlined composite pipeline with flange for liquid oxygen environment comprises a connecting section and a pipeline section; the connecting section comprises a flange layer and a sealing groove, the flange layer is made of a carbon fiber woven cloth impregnated with a compound epoxy resin, and the sealing groove is arranged on the end face of the flange layer for end face sealing; the pipeline section comprises an impermeable layer, a transition layer and a reinforcing layer from the inside to the outside, the impermeable layer is obtained by curing the carbon fiber surface felt impregnated with a compound epoxy resin; the transition layer is formed by winding a carbon fiber woven cloth; the reinforcing layer is made by combining a carbon fiber woven cloth impregnated with a compound epoxy resin and a carbon fiber yarn through a laying and winding method.
[0102] The rubber content of the impregnated layer is 55%, and the rubber content of the reinforcing layer and the flange layer is 25% after being impregnated; the transition layer is formed by circumferentially winding two layers of carbon fiber woven cloth.
[0103] The composite epoxy resin is the same as that in Example 1.
[0104] The method for preparing the composite material pipeline comprises the following steps:
[0105] (1) Install the core mold on the winding machine, spray the release agent on the surface of the core mold, and leave it for 10 hours after spraying;
[0106] (2) The carbon fiber surface felt is impregnated with a compound epoxy resin and then pre-cured. After the pre-curing is completed, the carbon fiber surface felt is taken out and laid flat on the surface of the core mold, and rolled into a cylinder as the mold rotates to form an impermeable layer;
[0107] (3) After the pre-curing of the anti-seepage layer is completed, two layers of carbon fiber woven fabrics are sequentially fastened on the outer surface of the anti-seepage layer by a circumferential winding method to form a transition layer;
[0108] (4) Continue to lay the composite epoxy resin impregnated carbon fiber woven cloth by circumferential fiber laying and winding to lay several reinforcement layers and flange layers. After the winding is completed, the pipeline is vacuumed and high-temperature cured by vacuuming to finally form a composite material pipeline.
[0109] Wherein, in step (2), the pre-curing temperature is 90° C. and the pre-curing time is 1.5 h;
[0110] Step (4) also includes:
[0111] a. First lay a layer of carbon fiber woven cloth with straight flange impregnated with composite epoxy resin, and then lay the reinforcement layer in the circumferential direction;
[0112] b. There are 8 reinforcement layers in total. After each reinforcement layer is laid, 25 layers of carbon fiber woven cloth impregnated with composite epoxy resin need to be laid to gradually form the flange layer;
[0113] c. Repeat steps a and b three times, cutting off the excess part at the edge of the flange each time to finally form a flange layer.
[0114] The vacuum degree of step (4) is 0.1-0.3 mbar, and the high temperature curing is firstly to uniformly heat from 30°C to 90°C within 60 minutes and keep it warm for 2 hours; then to uniformly heat to 120°C within 60 minutes and keep it warm for 4 hours; finally to uniformly heat to 160°C within 60 minutes and keep it warm for 3 hours.
[0115] Example 4
[0116] The difference between Example 4 and Example 1 is that the glue content of the anti-seepage layer after impregnation is 60%, and the glue content of the reinforcement layer after impregnation is 20%.
[0117] Comparative Example 1
[0118] The difference between Comparative Example 1 and Example 1 is that there is no transition layer in Comparative Example 1.
[0119] Comparative Example 2
[0120] The difference between Comparative Example 2 and Example 1 is that the anti-seepage layer in Comparative Example 2 is made of ordinary carbon fiber woven cloth.
[0121] Comparative Example 3
[0122] The difference between Comparative Example 3 and Example 1 is that ordinary bisphenol A epoxy resin is used in Comparative Example 3.
[0123] Comparative Example 4
[0124] The difference between Comparative Example 4 and Example 1 is that the anti-seepage layer in Comparative Example 4 does not undergo a pre-curing step.
[0125] Comparative Example 5
[0126] The difference between Comparative Example 5 and Example 1 is that in step (4) of Comparative Example 5, after laying the reinforcement layer, 80 layers of carbon fiber woven cloth impregnated with composite epoxy resin are directly laid on the right-angle section to form the flange layer.
[0127] Experimental example
[0128] The composite material pipelines prepared in Examples 1-4 and Comparative Examples 1-5 were respectively subjected to liquid oxygen compatibility and leakage rate tests.
[0129] 1. Liquid oxygen compatibility test: Liquid oxygen impact test is carried out according to the liquid oxygen compatibility evaluation standard of QJ3177-2003 standard. The liquid oxygen impact standard requires more than 98J. Each group is subjected to 20 independent impacts, and the energy is gradually increased each time for testing to obtain the maximum impact energy (J) that can be tolerated. If there is no sensitive reaction (such as sparks, charring, explosion, combustion, etc.) after 20 impact tests, it means that the material is compatible with liquid oxygen. If there is a sensitive reaction after 20 impact tests, 40 impact tests are carried out. If there is no sensitive reaction after 40 impact tests, it is also considered to be compatible with liquid oxygen.
[0130] 2. Helium mass spectrometer leak test: According to GB / T 13979-1992, the pipeline is tested for leakage rate at 2MPa by helium mass spectrometer at room temperature. The experimental results are shown in Table 1.
[0131] Table 1 Test results
[0132]
[0133]
[0134] In summary, the composite material pipeline prepared by the raw materials and methods defined in this application can withstand a liquid oxygen shock of up to 160J without flash, explosion or combustion. In the case of high liquid oxygen compatibility, the overall leakage rate of the pipeline is no more than 1×10 -4 Pa·m 3 / s, with good sealing performance, it can meet the low-temperature anti-seepage requirements and pressure-bearing requirements of liquid oxygen transportation.
[0135] The results show that the impact energy in Example 4 decreases and the leakage rate increases. Experimental analysis shows that this is because the excessive resin in the anti-seepage layer makes it relatively fragile and prone to cracks or breakage, affecting its anti-seepage performance and the stability of the overall structure; at the same time, due to the reduction in the glue content of the reinforcement layer, the bonding force between the carbon fiber and the resin is weakened, affecting the overall mechanical properties.
[0136] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0137] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A large-diameter, unlined composite material pipeline with flange for liquid oxygen environment, characterized in that: Including connecting sections and pipeline sections; The connecting section comprises a flange layer and a sealing groove, wherein the flange layer is made of a carbon fiber woven cloth layer impregnated with a composite epoxy resin, and the sealing groove is arranged on the end face of the flange layer for end face sealing; The pipeline section includes an impermeable layer, a transition layer and a reinforcement layer from the inside to the outside. The impermeable layer is obtained by curing the carbon fiber surface felt impregnated with a composite epoxy resin; the transition layer is formed by winding a carbon fiber woven cloth; the reinforcement layer is made by combining a carbon fiber woven cloth impregnated with a composite epoxy resin and a carbon fiber yarn through laying and winding.
2. The composite material pipeline according to claim 1, characterized in that: The anti-seepage layer has a glue content of 45-55% after impregnation, and the reinforcement layer and the flange layer have a glue content of 25-35% after impregnation; The transition layer is formed by hoop-winding two layers of carbon fiber woven fabric.
3. The composite material pipeline according to claim 1, characterized in that: The composite epoxy resin is prepared from the following raw materials in parts by weight: 80-100 parts of composite epoxy resin, 5-10 parts of composite nanofiller, 10-20 parts of ether diluent, 5-15 parts of flame retardant and 30-50 parts of amine curing agent; The compound epoxy resin comprises a bromine-containing epoxy resin, and the composite nano-filler comprises at least two silane-modified nano-materials.
4. The composite material pipeline according to claim 3, characterized in that: The compound epoxy resin also includes polyimide and meta-phenylenediamine; the weight ratio of the bromine-containing epoxy resin to the polyimide is (2-4):1, and the amount of meta-phenylenediamine used is 2-5% of the epoxy equivalent of the bromine-containing epoxy resin; The bromine-containing epoxy resin includes brominated bisphenol A epoxy resin or brominated bisphenol F epoxy resin.
5. The composite material pipeline according to claim 3, characterized in that: The composite nano filler comprises modified boron nitride nanotubes and modified alumina nanosheets in a weight ratio of 1:(2-5).
6. The composite material pipeline according to claim 3, characterized in that: The flame retardant is a phosphoric acid acrylate monomer containing a double bond.
7. The composite material pipeline according to claim 3, characterized in that: The amine curing agent is one of meta-phenylenediamine and 4,4'-diaminodiphenyl ether.
8. The composite material pipeline according to claim 3, characterized in that: The ether diluent includes one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, phenyl glycidyl ether and 4-tert-butylphenyl glycidyl ether.
9. A method for preparing a composite material pipeline according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Install the core mold on the winding machine, spray the release agent on the surface of the core mold, and leave it for 5-10 hours after spraying; (2) The carbon fiber surface felt is impregnated with a composite epoxy resin and then pre-cured. After the pre-curing is completed, the carbon fiber surface felt is taken out and laid flat on the surface of the core mold, and rolled into a cylinder as the mold rotates to form an impermeable layer; (3) After the pre-curing of the anti-seepage layer is completed, two layers of carbon fiber woven fabrics are sequentially fastened on the outer surface of the anti-seepage layer by a circumferential winding method to form a transition layer; (4) Continue to lay the composite epoxy resin impregnated carbon fiber woven cloth by circumferential fiber laying and winding to lay several reinforcement layers and flange layers. After the winding is completed, vacuum the pipeline and perform high-temperature curing to finally form the composite material pipeline.
10. The preparation method according to claim 9, characterized in that: In step (2), the pre-curing temperature is 50-90° C. and the pre-curing time is 1.5-2 h; Step (4) also includes: a. First lay a layer of carbon fiber woven cloth with straight flange impregnated with composite epoxy resin, and then lay the reinforcement layer in the circumferential direction; b. The number of reinforcement layers is 5-8 in total. After each reinforcement layer is laid, 15-25 layers of carbon fiber woven cloth impregnated with composite epoxy resin need to be laid to gradually form the flange layer; c. Repeat steps a and b 3-4 times, cutting off the excess part at the edge of the flange each time to finally form a flange layer.
Citation Information
Cited By
Prepreg cloth processing device and method for carbon fiber tube
CN120439587A
Low-temperature medium leakage prevention carbon fiber composite material with self-repairing and self-adaptive sealing functions as well as preparation method and application of low-temperature medium leakage prevention carbon fiber composite material
CN121375156A
Low-temperature media leakage resistant carbon fiber composite material with self-healing and adaptive sealing functions, its preparation method and application
CN121375156B
Resin glue solution, pressurized conveying gas cylinder used in liquid oxygen tank, manufacturing method of pressurized conveying gas cylinder and liquid rocket
CN121673765A
Nonmetal hydrogen conveying pipeline and preparation method thereof
CN122447562A