UV light-cured modified polyurethane acrylate water-based paint, preparation method and application of UV light-cured modified polyurethane acrylate water-based paint
By using thiol compounds and glucose oxidase and glucose to eliminate oxygen polymerization resistance system during UV photocuring, combined with photoinitiators and additives, the oxygen polymerization problem is solved, and the polymerization rate and monomer conversion rate are improved. , realizes excellent mechanical and heat resistance of the paint, and is suitable for automotive leather.
Patent Information
- Application Number
- CN202410902124.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-12
AI Technical Summary
During the existing UV photocuring process, oxygen polymerization resistance and uneven cross-linking are prone to occur, resulting in slow polymerization rate and low monomer conversion rate, which affects the mechanical and heat resistance of the coating.
UV photocuring modified polyurethane acrylate water-based coating is prepared by mixing thiol compounds with two different oxygen-elimination and polymerization systems, combining photoinitiators and additives. , to form excellent mechanical and heat resistance.
Effectively reduces the oxygen resistance effect during UV photocuring, improves the polymerization rate and monomer conversion rate, reduces odor, and ensures stable material performance. It is suitable for automotive leather coatings.
Smart Images

Figure BDA0004930761630000051 
Figure BDA0004930761630000061 
Figure BDA0004930761630000062
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based coatings for automotive leather, and in particular to a UV light-cured modified polyurethane acrylate water-based coating, a preparation method and application thereof. Background Art
[0002] Waterborne polyurethane has been widely used in various industrial fields, especially in the coating field, due to its great advantages in environmental protection.
[0003] However, waterborne polyurethanes are mostly linear structures and cannot form a cross-linked network structure, so their heat resistance is poor. When used in the field of automotive leather coatings, a problem arises: poor heat resistance leads to a significant reduction in the service life of automotive leather. Based on this, since acrylates have excellent weather resistance and physical and mechanical properties, using acrylate emulsions to modify polyurethane to increase the cross-linking degree of waterborne polyurethane, thereby improving the physical and mechanical properties and heat resistance of the coating, is a good research hotspot.
[0004] For example, prior art 1: Chinese patent CN 114410174 B discloses a high-performance water-based acrylic polyurethane coating and a preparation method thereof. The high-performance water-based acrylic polyurethane coating is composed of the following raw materials in parts by mass: 200 to 300 parts of vegetable oil acid-modified epoxy-acrylic resin, 50 to 150 parts of blocked water-based polyurethane, 0.25 to 1 part of defoaming agent, 0.25 to 2.5 parts of dispersant, and 50 to 150 parts of pigments and fillers.
[0005] Prior art 1 combines water-based acrylic resin and water-based polyurethane resin to meet environmental protection requirements while making high-performance water-based acrylic polyurethane coatings with low VOC content, high crosslinking density of the paint film, stable storage at room temperature, and excellent water resistance, adhesion, hardness, toughness, drying speed, salt spray resistance, impact resistance, gloss and other properties; at the same time, paragraphs 0009 and 0010 of the specification of prior art 1 record the preparation method of vegetable oil acid modified epoxy-acrylic resin: vegetable oil acid, epoxy resin, and catalyst I are added to a reactor, N2 is introduced, stirring is started at 150r / min, the temperature is raised to 120-180°C, and the reaction is performed for 2-4h to generate epoxy ester; then solvent I is added, and the uniformly mixed acrylic monomer and initiator are dripped into the reactor at a uniform speed, and the mixture is stirred at 100-1 The mixture is further reacted at 40°C for 3 to 6 hours; then the temperature is lowered to 50 to 80°C, a neutralizing agent I is added for neutralization for 15 to 30 minutes, and deionized water is added dropwise under high-speed stirring at 2000 to 3000 r / min to obtain a vegetable oil acid-modified epoxy-acrylic resin; the vegetable oil acid is one or more of linoleic acid, ricinoleic acid, dehydrated ricinoleic acid, soybean oil acid, and eleostearic acid; the epoxy resin is one or more of bisphenol A type epoxy resin E-06, E-12, E-20, and E-44; the catalyst I is one or a combination of tetrabutylammonium bromide and zinc oxide; the initiator is one or more of azobisisobutyronitrile, benzoyl peroxide, and tert-butyl perbenzoate; the solvent I is one or more of n-butanol, propylene glycol methyl ether, propylene glycol butyl ether, and sec-butanol.
[0006] The technical solution of prior art 1 provides certain technical inspiration in the production direction of coatings used for automotive leather, allowing technical personnel in this field to consciously combine water-based acrylic resins and water-based polyurethane resins to produce coatings for automotive leather.
[0007] However, in the actual application of automotive leather coatings, it was found that since automotive leather coatings are currently cured by UV light, the technical solution of prior art 1 will have a problem, that is, it is prone to oxygen inhibition, uneven cross-linking and other phenomena, resulting in slow polymerization rate and low monomer conversion rate, which ultimately affects the mechanical, heat resistance and other properties of the coating.
[0008] In the prior art, there are many ways to reduce oxygen inhibition, such as changing the photoinitiator, but this often increases the cost; directly adding a tertiary amine co-initiator, but this often leads to a darker color and affects the appearance; now the effect of oxygen inhibition is often reduced by introducing antioxidant inhibitory groups, such as: generating tertiary amine acrylates through the Michael addition reaction of tertiary amines and hydroxy acrylates, and introducing active amine groups, but this usually also affects the color of the cured film; there is also the introduction of thiols to reduce oxygen inhibition, but this method often has problems with excessive odor and poor storage stability.
[0009] Therefore, the technical problem to be solved by the present invention is: how to further reduce the oxygen inhibition effect during UV light curing and effectively improve the polymerization rate and monomer conversion rate of UV light curing. Summary of the invention
[0010] One of the purposes of the present invention is to provide a UV light-curable modified polyurethane acrylate water-based coating, which can effectively reduce the oxygen inhibition effect during UV light curing and improve the polymerization rate and monomer conversion rate of UV light curing.
[0011] Another object of the present invention is to provide a method for preparing a UV light-curing modified polyurethane acrylate water-based coating, wherein the prepared UV light-curing modified polyurethane acrylate water-based coating has excellent mechanical and heat-resistant properties.
[0012] At the same time, the present invention also provides an application of a UV light-cured modified polyurethane acrylate water-based coating, which has excellent application prospects when applied to automotive leather due to its advantages of water-based environmental protection, good mechanical properties and good heat resistance.
[0013] To achieve the above-mentioned object, the present invention provides a UV light-curing modified polyurethane acrylate water-based coating, which comprises the following components in parts by weight: 80-95 parts of water-based polyurethane acrylate emulsion, 1-2 parts of thiol compounds, 1-2 parts of glucose oxidase, 2-3 parts of glucose, 1-4 parts of photoinitiator, and 1-10 parts of auxiliary agent.
[0014] Preferably, the solid content of the aqueous polyurethane acrylate emulsion is 40-60%.
[0015] Preferably, the thiol compound is at least one of mercaptoethanol, mercaptopropanol and dodecyl mercaptan.
[0016] Preferably, the photoinitiator is at least one of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxy-cyclohexyl phenyl ketone, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0017] Furthermore, the auxiliary agent includes at least one of a stabilizer, a matting agent, a defoaming agent, a leveling agent, and a plasticizer.
[0018] The present invention also provides a method for preparing a UV light-cured modified polyurethane acrylate water-based coating, comprising the following steps:
[0019] Step 1: preparing waterborne polyurethane acrylate emulsion;
[0020] Step 2: Add thiol compounds, glucose oxidase, glucose, and photoinitiator to the aqueous polyurethane acrylate emulsion, and stir to mix evenly;
[0021] Step 3: Add additives and stir evenly to obtain UV light-cured modified polyurethane acrylate water-based coating.
[0022] Furthermore, the specific operations of step 1 are:
[0023] Step a: prepare the raw materials of 60-80 parts of diisocyanate, 90-110 parts of polyol, 0.1-4 parts of diol, 10-25 parts of carboxyl diol, 1-20 parts of hydroxy acrylate, 20-55 parts of acrylate functional monomer, 5-20 parts of triethylamine, and appropriate amount of deionized water;
[0024] Step b: reacting diisocyanate, polyol, diol and carboxyl diol to generate an NCO-containing prepolymer;
[0025] Step c: reacting the NCO-containing prepolymer with hydroxy acrylate to consume NCO, and then adding acrylate functional monomer for copolymerization;
[0026] Step d: After the copolymerization is completed, triethylamine is added to carry out neutralization reaction for 20-30 minutes, and then deionized water is added for emulsification for 45-50 minutes, and then evaporated to obtain a waterborne polyurethane acrylate emulsion.
[0027] Furthermore, the specific operation of step b is: prepolymerizing diisocyanate, polyol, diol and carboxyl diol at 75-95° C. to generate an NCO-containing prepolymer.
[0028] Furthermore, the specific operation of step c is: cooling the NCO-containing prepolymer to 45° C., adding hydroxy acrylate and heating to 60-65° C. to react for 4 hours, and then adding acrylate functional monomer and reacting at 70-80° C. for 2 hours.
[0029] Preferably, the diisocyanate is at least one of diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, and xylylene diisocyanate.
[0030] Preferably, the polyol can be selected from at least one of adipic acid-based polyester polyol, polyether polyol, polycaprolactone polyol, and polycarbonate polyol.
[0031] Preferably, the diol can be selected from at least one of ethylene glycol, 1,4-butanediol and neopentyl glycol.
[0032] Preferably, the carboxyl diol can be selected from at least one of dimethylol propionic acid and dimethylol butyric acid.
[0033] Preferably, the acrylate functional monomer may be at least one of methyl acrylate, ethyl acrylate and glycidyl methacrylate.
[0034] The present invention further provides an application of a UV light-cured modified polyurethane acrylate water-based paint, which is applied to automotive leather.
[0035] Beneficial Effects
[0036] Compared with the prior art, the present invention has at least the following advantages:
[0037] (1) The present invention uses a thiol compound mixed with glucose oxidase and glucose, two different oxygen inhibition elimination systems, to effectively solve the oxygen inhibition effect produced by the photopolymerization reaction, while synergistically improving the polymerization rate and monomer conversion rate of UV light curing;
[0038] (2) The invention effectively reduces the amount of thiol compounds used by adding glucose oxidase and glucose to form an oxygen inhibition system, thereby avoiding the presence of unreacted thiol groups in the polymer network and effectively ensuring that the material properties will not be reduced due to unreacted thiol groups;
[0039] (3) The present invention adopts a mixture of thiol compounds with two different oxygen inhibition systems, glucose oxidase and glucose, which not only effectively solves the oxygen inhibition effect produced by the photopolymerization reaction, but also reduces the odor of UV light-cured modified polyurethane acrylate water-based coating, and has excellent application prospects when used for automotive leather. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with the embodiments, but it does not constitute any limitation to the present invention. Any limited number of modifications made within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0041] In order to explain the technical content of the present invention in detail, further description is given below in conjunction with the implementation modes.
[0042] In the technical scheme of the present invention, the raw materials used can be purchased from the market; in the following examples and comparative examples, the isophorone diisocyanate and 1,4-butanediol are purchased from Guangzhou Haoyi New Materials Technology Co., Ltd., the polyether polyol DL2000 is purchased from Tonglan New Energy Technology Development (Shandong) Group Co., Ltd., dimethylolpropionic acid is purchased from Shandong Xiaoqing New Chemical Co., Ltd., hydroxyethyl acrylate is purchased from Hubei Xinyuhong Biomedicine Technology Co., Ltd., triethylamine is purchased from Hefeng New Energy Co., Ltd., dodecyl mercaptan is purchased from Jinan Junteng Chemical Co., Ltd., glucose oxidase is purchased from Hunan Yunbang Biotechnology Co., Ltd., glucose is purchased from Gongyi Longda Water Treatment Materials Co., Ltd., 2-hydroxy-2-methyl-1-phenyl-1-propanone is purchased from Shandong Xinghai Chemical Co., Ltd., and the defoamer SN-6725, wetting agent SN-4727, and leveling agent SN4034 are all purchased from Shanghai Shenzhu Chemical Technology Co., Ltd.
[0043] In the following examples and comparative examples, unless otherwise specified, parts and % are parts by weight and percentage by weight, respectively.
[0044] In the following examples and comparative examples, the aqueous polyurethane acrylate emulsions are prepared by the following steps:
[0045] Step a: prepare the raw materials of 70 parts of isophorone diisocyanate, 100 parts of polyether polyol DL2000, 3 parts of 1,4-butanediol, 18 parts of dimethylol propionic acid, 12 parts of hydroxy acrylate, 45 parts of ethyl acrylate, 5-20 parts of triethylamine, and an appropriate amount of deionized water;
[0046] Step b: prepolymerizing isophorone diisocyanate, polyether polyol DL2000, 1,4-butanediol and dimethylol propionic acid at 90° C. to generate an NCO-containing prepolymer;
[0047] Step c: cool the NCO-containing prepolymer to 45°C, add hydroxy acrylate and heat to 65°C for reaction for 4h, then add ethyl acrylate and react at 75°C for 2h;
[0048] Step d: After the copolymerization is completed, triethylamine is added to carry out neutralization reaction for 30 minutes, and then deionized water is added for emulsification for 50 minutes, and then evaporated to obtain an aqueous polyurethane acrylate emulsion with a solid content of 40%.
[0049] According to the formula in Table 1, a UV light-curing modified polyurethane acrylate water-based coating is prepared. The preparation method is as follows:
[0050] Step 1: Add dodecyl mercaptan, glucose oxidase, glucose and photoinitiator to the aqueous polyurethane acrylate emulsion, and stir to mix evenly;
[0051] Step: 2: Add additives and stir evenly to obtain UV light-cured modified polyurethane acrylate water-based coating.
[0052] Table 1 UV light-cured modified polyurethane acrylate water-based coating formula
[0053]
[0054]
[0055] Performance Testing
[0056] 1. Polymerization rate and monomer conversion rate during photocuring reaction
[0057] Test method: Differential thermal scanning was used to study the reaction process.
[0058] The UV light-curable modified polyurethane acrylate water-based coatings obtained in Examples 1-4 and Comparative Examples 1-4 were subjected to a light-curing reaction, and the polymerization rate and monomer conversion rate during the light-curing reaction were obtained by using differential thermal scanning, as shown in Table 1;
[0059] Table 1 Photocuring polymerization rate and monomer conversion rate of Examples 1-4 and Comparative Examples 1-4
[0060]
[0061] According to the results in Table 1, we can see that:
[0062] According to the data of Examples 1-4, the present invention uses a thiol compound mixed with glucose oxidase and glucose, two different oxygen inhibition elimination systems, to effectively synergistically improve the photocuring polymerization rate and monomer conversion rate of the water-based coating, and synergistically eliminate the effects of oxygen inhibition during UV photocuring.
[0063] According to the data comparison of Example 4 and Comparative Examples 1 and 2, it can be seen that the effect of simply using thiol compounds or glucose oxidase and glucose to eliminate the oxygen inhibition effect in the UV photocuring process of water-based coatings is significantly reduced compared with the technical solution of the present invention. This shows that the present invention uses thiol compounds and glucose oxidase and glucose, two different oxygen inhibition elimination systems, to mix to produce a synergistic effect of improving the photocuring polymerization rate and monomer conversion rate of water-based coatings.
[0064] 2. Mechanical properties
[0065] Test method: Hardness is tested according to GB / T6739, and impact strength is tested according to GB / T 1732.
[0066] The mechanical properties of the UV light-cured modified polyurethane acrylate water-based coatings obtained in Examples 1-4 and Comparative Examples 1-4 were tested, and the results are shown in Table 2;
[0067] Table 2 Mechanical properties of UV light-cured modified polyurethane acrylate water-based coatings obtained in Examples 1-4 and Comparative Examples 1-4
[0068] hardness Impact strength (kg cm) Example 1 5H 61 Example 2 4H 58 Example 3 4H 56 Example 4 4H 58 Comparative Example 1 HB 44 Comparative Example 2 3H 50 Comparative Example 3 F 46 Comparative Example 4 2H 50
[0069] According to Table 2, we can see that:
[0070] According to Example 4 and Comparative Example 1, the present invention uses a thiol compound mixed with two different oxygen-eliminating inhibition systems, glucose oxidase and glucose, to avoid the problem of material performance degradation caused by residual thiol compounds; and the use of excessive thiol compounds in Comparative Example 3 will also cause similar problems. Combined with Table 1, although the thiol compound used in Comparative Example 3 is mixed with two different oxygen-eliminating inhibition systems, glucose oxidase and glucose, which can further improve the photocuring polymerization rate and monomer conversion rate, the excessive thiol compound causes unreacted thiol groups to exist in the polymer network, which significantly reduces the mechanical properties of the water-based coating.
[0071] According to the data comparison between Example 4 and Comparative Example 2 and combined with the results of Table 1, it can be seen that the photocuring polymerization rate and monomer conversion rate of the oxygen inhibition elimination system using glucose oxidase and glucose in Comparative Example 2 are significantly reduced compared with the technical solution of the present invention, thereby affecting the mechanical properties of the water-based coating.
[0072] According to the comparison of the data of Example 4 and Comparative Example 4, it can be seen that in the technical scheme of mixing thiol compounds with two different oxygen-eliminating inhibition systems of glucose oxidase and glucose, excessive use of the oxygen-eliminating inhibition system of glucose oxidase and glucose will lead to a decrease in the mechanical properties of the water-based coating. The reason is that excessive use of the oxygen-eliminating inhibition system of glucose oxidase and glucose may result in part of the thiol compounds not participating in the reaction, and unreacted thiol groups exist in the polymer network, which significantly reduces the mechanical properties of the water-based coating.
[0073] The embodiments presented herein are only embodiments selected according to the combination of all possible embodiments. The appended claims should not be limited by the embodiments describing the present invention. Some numerical ranges used in the claims include sub-ranges therein, and the changes in these ranges should also be covered by the appended claims.
Claims
1. A UV light-cured modified polyurethane acrylate water-based coating, It is characterized in that The composition comprises the following components by weight: 80-95 parts of waterborne polyurethane acrylate emulsion, 1-2 parts of thiol compound, 1-2 parts of glucose oxidase, 2-3 parts of glucose, 1-4 parts of photoinitiator and 1-10 parts of auxiliary agent.
2. The UV light-curable modified polyurethane acrylate water-based coating according to claim 1, It is characterized in that The solid content of the aqueous polyurethane acrylate emulsion is 40-60%.
3. The UV light-curable modified polyurethane acrylate water-based coating according to claim 1, It is characterized in that The thiol compound is at least one of mercaptoethanol, mercaptopropanol and dodecyl mercaptan.
4. The UV light-curable modified polyurethane acrylate water-based coating according to any one of claims 1 to 3, It is characterized in that The photoinitiator is at least one of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxy-cyclohexyl phenyl ketone, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
5. The UV light-curable modified polyurethane acrylate water-based coating according to any one of claims 1 to 3, It is characterized in that The auxiliary agent includes at least one of a stabilizer, a matting agent, a defoaming agent, a leveling agent, and a plasticizer.
6. A method for preparing a UV light-curable modified polyurethane acrylate water-based coating as claimed in any one of claims 1 to 5, It is characterized in that The steps include: Step 1: preparing waterborne polyurethane acrylate emulsion; Step 2: Add thiol compound, glucose oxidase, glucose and photoinitiator to the aqueous polyurethane acrylate emulsion, and stir to mix evenly; Step 3: Add additives and stir evenly to obtain UV light-cured modified polyurethane acrylate water-based coating.
7. The method for preparing the UV light-curable modified polyurethane acrylate water-based coating according to claim 6, It is characterized in that The specific operations of step 1 are: Step a: prepare the raw materials of 60-80 parts of diisocyanate, 90-110 parts of polyol, 0.1-4 parts of diol, 10-25 parts of carboxyl diol, 1-20 parts of hydroxy acrylate, 20-55 parts of acrylate functional monomer, 5-20 parts of triethylamine, and appropriate amount of deionized water; Step b: reacting diisocyanate, polyol, diol and carboxyl diol to generate an NCO-containing prepolymer; Step c: reacting the NCO-containing prepolymer with hydroxy acrylate to consume NCO, and then adding acrylate functional monomer for copolymerization; Step d: After the copolymerization is completed, triethylamine is added to carry out neutralization reaction for 20-30 minutes, and then deionized water is added for emulsification for 45-50 minutes, and then evaporated to obtain a waterborne polyurethane acrylate emulsion.
8. The method for preparing the UV light-curable modified polyurethane acrylate water-based coating according to claim 7, It is characterized in that The specific operation of step b is: prepolymerizing diisocyanate, polyol, diol and carboxyl diol at 75-95° C. to generate NCO-containing prepolymer.
9. The method for preparing the UV light-curable modified polyurethane acrylate water-based coating according to claim 7, It is characterized in that The specific operation of step c is: cooling the NCO-containing prepolymer to 45° C., adding hydroxy acrylate and heating to 60-65° C. to react for 4 hours, and then adding acrylate functional monomer and reacting at 70-80° C. for 2 hours.
10. An application of the UV light-curable modified polyurethane acrylate water-based coating as claimed in any one of claims 1 to 5, It is characterized in that Used in automotive leather.
Citation Information
Patent Citations
Ultraviolet-cured waterborne polyurethane-acrylate glossy leather finishing agent
CN106752880A
An acrylate modified polyurethane emulsion and a preparing method thereof
CN106916254A
Ultraviolet light hybrid light curing waterborne polyurethane acrylate and preparation method and application thereof
CN108948321A
UV waterproof leak-repairing coating as well as preparation method and application thereof
CN113549394A
Preparation of ultraviolet-curing paint and application of ultraviolet-curing paint as isolation protective paint for pre-paved high-polymer waterproof sheet
CN114045085A
Cited By
Environment-friendly UV curing coating and preparation process thereof
CN120349721A