Collision-resistant waterproof foam rubber and preparation method thereof
By using waterproof foam glue combined with modified silica and thermoplastic copolymer in automotive sealing systems, the problem of seal failure of foamed silicone after compression deformation is solved, achieving high-performance collision resistance, flame retardant and waterproofing effects , suitable for automotive seals and fire-retardant materials.
Patent Information
- Application Number
- CN202411078348.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
In existing automotive sealing systems, foamed silicone can easily lead to seal failure after compression and deformation, and lack of waterproofing performance, which increases maintenance costs.
A collision-resistant waterproof foam glue is adopted, which consists of a composite release layer, a flame-retardant double-sided adhesive layer, a cotton paper layer and a foamed silicone layer. The combination of modified silica and thermoplastic copolymer can improve the material's Compatibility and compression resistance, forming a spatial network structure to enhance flame retardant and waterproofing.
It has achieved excellent collision resistance, good flame retardant effect and good waterproof performance of foam glue. It is suitable for high-performance sealing and fire-resistant shock-absorbing buffer layers, significantly improving compression and impact toughness, and maintaining long-term use. Soft and elastic properties.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of adhesive products, and particularly relates to a collision-resistant and waterproof foam adhesive and a preparation method thereof. Background Art
[0002] The sealing system of a car is an important part of the design and development of car doors and windows. The sealing system affects the sealing performance of the entire vehicle and the ease of opening and closing the doors and windows. At present, the automotive industry widely uses adhesives and tapes to replace traditional welding, riveting and other processes. They are used for the direct installation, fixation and sealing of the sealing strip and the car body, which brings better installation adjustability, body conformity and sealing to the sealing strip parts. Among all types of automotive double-sided tapes, acrylic foam tape is the most widely used type. Acrylic foam pressure-sensitive adhesive uses high-density elastic foam material as the base material. Because of its good bonding performance, sealing performance and buffering and shock-absorbing performance, it is widely used in the fixing of automotive exterior parts. In addition to certain requirements for the peel strength of the tape, high-performance acrylic foam pressure-sensitive adhesive should also have excellent flame retardant and weather resistance.
[0003] Foamed silicone refers to adding a foaming agent to the rubber material. During the vulcanization process, the foaming agent decomposes at high temperature to produce bubbles. The bubbles are wrapped in the silicone rubber to form foamed silicone. It not only maintains the original excellent properties of silicone, but also has the characteristics of heat insulation, sound insulation, shock absorption, and light weight. However, when used in conjunction with acrylic foam tape in the field of automotive sealing, the problem of sealing failure often occurs due to large compression deformation. The lack of collision resistance hinders its long-term use and increases maintenance costs.
[0004] The invention patent with application number 201410837218.2 discloses a method for preparing a modified polysiloxane / two-component foamed silicone composite material. The present invention discloses a method for preparing a modified polysiloxane / two-component foamed silicone composite material. First, component A and component B are prepared, and then boric acid and terminal hydroxyl polydimethylsiloxane are used to prepare boric acid-modified terminal hydroxyl polydimethylsiloxane, and the boric acid-modified terminal hydroxyl polydimethylsiloxane is first mixed with component A, and then the obtained mixture is mixed with component B for cross-linking and foaming reaction to obtain the modified polysiloxane / two-component foamed silicone composite material prepared by the invention. When the modified polysiloxane / two-component foamed silicone composite material is subjected to shear or impact, the boric acid-modified polysiloxane distributed in the material in a dispersed phase can absorb and dissipate a part of the energy through a sharp change in its viscosity, thereby achieving the reinforcement of the two-component foamed silicone matrix. After the impact, the non-destructive deformation can be restored, but the waterproof performance of the two-component composite material still has room for improvement.
[0005] Therefore, it is particularly important for the present invention to provide a collision-resistant and waterproof foam adhesive. Summary of the invention
[0006] In view of the defects of the prior art, the present invention provides a collision-resistant and waterproof foam adhesive and a preparation method thereof. The foam adhesive provided by the present invention is a high-performance foam adhesive with excellent collision resistance, good flame retardant effect and waterproofness, and is suitable for use as a shock-absorbing buffer layer for various high-performance sealing, protection and fireproof materials.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] On one hand, the present invention provides a collision-resistant and waterproof foam adhesive, which comprises a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer in sequence;
[0009] Wherein, the thickness of the foam glue is 2 to 15 mm.
[0010] Another aspect of the present invention provides a method for preparing a collision-resistant and waterproof foam adhesive, comprising the following steps: coating a flame-retardant double-sided adhesive on the release layer to form a first flame-retardant double-sided adhesive layer, the dry weight of which is 35 to 37.5 g / m 2 , and then a cotton paper layer is attached on the first flame retardant double-sided adhesive layer, and then a flame retardant double-sided adhesive is applied on the cotton paper layer to form a second flame retardant double-sided adhesive layer, the dry weight of which is 35-37.5g / m 2 Then, a foamed silica gel is coated on the second flame retardant double-sided adhesive layer to form a foamed silica gel layer, and the foamed silica gel layer is cured at 20-50° C. to obtain the collision-resistant and waterproof foam adhesive.
[0011] In some embodiments of the present invention, the flame retardant double-sided adhesive comprises the following raw materials in parts by weight: 20 to 50 parts of acrylic prepolymer, 10 to 25 parts of adhesive, 3 to 10 parts of tackifying resin, 2 to 18 parts of first flame retardant, 1 to 5 parts of modified silica, and 3 to 5 parts of isocyanate curing agent.
[0012] In some embodiments of the present invention, the preparation steps of the modified silicon dioxide are as follows:
[0013] (1) Adding a composite silane coupling agent into a reactor, stirring and heating to 110-130° C. under an inert atmosphere, reacting for 4-7 hours, cooling to room temperature after the reaction is completed, and obtaining a modifier;
[0014] (2) Add solvent to another reactor, adjust the pH to 4-6, then add modifier, stir and mix at 40-60°C for 3-8h to obtain hydrolyzed modifier, then add silica, continue to heat to 60-70°C, set stirring conditions to 400-500 r / min, stir and react for 4-5h to obtain modified silica.
[0015] Preferably, the preparation steps of the modified silicon dioxide are as follows:
[0016] (1) Adding a composite silane coupling agent into a reactor, stirring and heating to 120° C. under an inert atmosphere, reacting for 5.5 hours, and cooling to room temperature after the reaction is completed to obtain a modifier;
[0017] (2) Add solvent to the reactor, add hydrochloric acid to adjust the pH to 5, then add modifier, stir and mix at 50°C for 5.5 hours to obtain hydrolyzed modifier, then add silica, continue to heat to 65°C, set the stirring condition to 450r / min, stir and react for 4.5 hours to obtain modified silica.
[0018] Preferably, the composite silane coupling agent is a combination of γ-methacryloxypropyltrimethylsilane and γ-glycidyloxypropyltrimethoxysilane, and the molar ratio of the two is (1-1.2):1.
[0019] Preferably, the solvent is a mixture of isobutanol and deionized water, with a mass ratio of 6:1.
[0020] Preferably, the amount of the solvent added is 30 to 50 times the total mass of the modifier and silica.
[0021] In some embodiments of the present invention, the mass ratio of the modifier to silicon dioxide is 1:(7-12).
[0022] Preferably, the mass ratio of the modifier to silicon dioxide is 1:9.5.
[0023] In some embodiments of the present invention, the mass ratio of the first flame retardant to the modified silica is 1:(0.2-0.5).
[0024] Preferably, the mass ratio of the flame retardant to the modified silica is 1:0.35.
[0025] Preferably, the acrylic prepolymer is an amino group-containing acrylic polymer resin, and has a viscosity of 10 to 38 Pa·s at 25°C.
[0026] Preferably, the adhesive is chloroprene rubber, and the tackifying resin is hydrogenated rosin.
[0027] Preferably, the first flame retardant is an organosilicon flame retardant.
[0028] Preferably, the isocyanate curing agent is isocyanate.
[0029] In some embodiments of the present invention, the preparation steps of the flame retardant double-sided adhesive are as follows: add acrylic prepolymer, adhesive, tackifying resin and first flame retardant into a reactor, add modified silica and mix evenly, then add isocyanate curing agent and mix thoroughly to obtain flame retardant double-sided adhesive.
[0030] In the prior art, silica is often added as a reinforcing filler to improve the comprehensive performance and stability of double-sided adhesive tape. However, due to the strong polarity of silica and its poor compatibility in the system, it is difficult to achieve full combination and thus play a reinforcing role. The present invention prepares an alkoxy modifier at both ends to graft-modify the silica surface. After hydrolysis, the alkoxy modifier reacts with the abundant active hydroxyl groups on the silica surface, thereby reducing the self-aggregation of silica and increasing compatibility. On the other hand, the applicant found that when the modified silica was added to the double-sided adhesive tape system and the mass ratio of the flame retardant component to the modified silica was controlled, the flame retardant properties of the colloid were unexpectedly improved. The possible reason is that the prepared modifier solves the self-aggregation of silica to achieve uniform dispersion and increase its compatibility with the system. At the same time, it exists in the colloid in a spatial network structure formed by particles that are interconnected but not directly in contact, and the flame retardant components in the coupling colloid play a synergistic flame retardant role.
[0031] In some embodiments of the present invention, the foamed silica gel comprises the following raw materials in parts by weight: 50 to 100 parts of modified organic siloxane, 10 to 35 parts of fumed silica, 0.6 to 2 parts of methyl hydrogenated silicone oil, 20 to 50 parts of a second flame retardant, 0.01 to 1.0 parts of a catalyst and 6 to 8 parts of hydrogenated silicone oil.
[0032] In some embodiments of the present invention, the preparation steps of the modified organosiloxane are as follows: add the organosiloxane to a reactor, add the thermoplastic copolymer, stir well, add the curing agent, stir and react at 80-90°C for 1-3h to obtain the modified organosiloxane.
[0033] Preferably, the preparation steps of the modified organosiloxane are as follows: adding the organosiloxane into a reactor, adding the thermoplastic copolymer, stirring well, adding the curing agent, stirring and reacting at 85° C. for 2 hours to obtain the modified organosiloxane.
[0034] Preferably, the mass ratio of the organosiloxane to the thermoplastic copolymer is (0.2-1):1.
[0035] Further preferably, the mass ratio of the organosiloxane to the thermoplastic copolymer is 0.6:1.
[0036] Preferably, the curing agent is butyl diphenylcarbamate, and the added amount is 10% of the mass of the organosiloxane.
[0037] Preferably, the organosiloxane is hydroxypolydimethylsiloxane, and the thermoplastic copolymer is thermoplastic copolymer TSM.
[0038] In some embodiments of the present invention, the preparation steps of the foamed silica gel are as follows: add the modified organic siloxane into the reactor, then add the fumed silica and the second flame retardant into the container, stir at 60-90°C for 0.8-1.6h, then stir in vacuum for 5-25min, reduce the temperature to 6-15°C, add the catalyst and mix evenly, then add the hydrogenated silicone oil, stir for 10-30min, and obtain the foamed silica gel.
[0039] Preferably, the preparation steps of the foamed silica gel are as follows: adding the modified organosiloxane into the reactor, then adding the fumed silica and the second flame retardant into the container, stirring at 75°C for 1.2 hours, then stirring under vacuum for 15 minutes, lowering the temperature to 10.5°C, then adding the catalyst and mixing evenly, then adding the hydrogenated silicone oil, stirring for 20 minutes, and obtaining the foamed silica gel.
[0040] Preferably, the particle size of the fumed silica is 5 to 30 nm, the second flame retardant is an organic silicon flame retardant, the catalyst is a platinum catalyst, and the hydrogen content of the hydrogen-containing silicone oil is 1 to 3%.
[0041] The present invention achieves the effect of foaming and expansion by introducing a thermoplastic copolymer into hydroxy polydimethylsiloxane for modification, and utilizes the temperature-sensitive expansion characteristics of the thermoplastic copolymer, and significantly improves the compressive effect and impact toughness of the foamed silica gel. The possible reason is that the helical structure of the polydimethylsiloxane main chain makes the chain easy to arrange itself, and the intermolecular force is weak, and it has excellent flexibility. When the closed-cell hollow structure is introduced to modify it, the interface interaction between the thermoplastic copolymer and the organic siloxane can achieve effective transfer of stress, and its gradual rupture under stress is reflected in the macroscopic softening behavior, and the direct fragmentation of the foamed silica gel is avoided by absorbing and dissipating energy; on the other hand, the applicant avoids the influence of agglomeration and accumulation caused by the expansion of the thermoplastic copolymer on the interface interaction of the modified object by regulating the mass ratio of the thermoplastic copolymer and the hydroxy polydimethylsiloxane, and reduces its influence on the hydrophobicity of the foamed silica gel, which improves the chemical stability of the foam glue.
[0042] Preferably, the release layer is a silicone release film with a thickness of 0.5 μm.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] (1) The foam adhesive provided by the present invention has excellent collision resistance, good flame retardant effect and good waterproof performance, and various high-performance sealing, protection and fireproof materials are used as shock-absorbing buffer layers;
[0045] (2) The impact-resistant and waterproof foam adhesive provided by the present invention is prepared by grafting and modifying the surface of silica with an alkoxy modifier at both ends, thereby reducing the self-aggregation of silica, increasing compatibility, and improving the comprehensive performance and stability of the double-sided adhesive;
[0046] (3) The collision-resistant and waterproof foam adhesive provided by the present invention adjusts the mass ratio of the flame retardant component and the modified silica, so that the modified silica can solve the self-aggregation phenomenon of silica to achieve uniform dispersion and increase its compatibility with the system. At the same time, the particles are connected to each other but not directly in contact with each other to form a spatial network structure in the colloid, and the flame retardant component in the coupling colloid plays a synergistic flame retardant role;
[0047] (3) The collision-resistant and waterproof foam adhesive provided by the present invention improves the interfacial interaction between the thermoplastic copolymer and the organosiloxane by introducing the thermoplastic copolymer into the modified organosiloxane, realizes the effective transfer of stress, and significantly improves the compressive effect and impact toughness of the foamed silica gel by absorbing and dissipating energy. On the other hand, by regulating the modification of the hydroxyl polydimethylsiloxane by the thermoplastic copolymer, the influence of agglomeration and accumulation of the thermoplastic copolymer on the interfacial interaction in the modified organosiloxane structure is avoided, thereby reducing its influence on the hydrophobicity of the foamed silica gel, and synergistically improving the chemical stability of the foam adhesive. DETAILED DESCRIPTION
[0048] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0049] If not otherwise specified, the reagents used below can be easily obtained from commercial companies. In the following preparation examples and embodiments, if not otherwise specified, amino-containing acrylic polymer resin was purchased from Jining Tangyi Chemical Co., Ltd., hydrogenated rosin was purchased from Beijing Haitongwei Technology Development Co., Ltd., silicone flame retardant was purchased from Guangdong Quansheng Chemical Co., Ltd., hydroxy polydimethylsiloxane, hydrogen-containing silicone oil and methyl hydrogen-containing silicone oil were all purchased from Dow Corning, USA, silicone release agent was purchased from Hubei Xinsihai Chemical Co., Ltd., platinum catalyst was purchased from Xiemei Chemical (Guangzhou) Co., Ltd., and thermoplastic copolymer TSM was purchased from Hefei Jieshijie New Materials Co., Ltd.
[0050] Preparation Example 1
[0051] The preparation steps of modified silica I are as follows:
[0052] (1) Add 1.1 mol of γ-methacryloxypropyltrimethylsilane and 1 mol of γ-glycidyloxypropyltrimethoxysilane into a reactor, stir and heat to 120° C. under a nitrogen atmosphere, react for 5.5 hours, and cool to room temperature after the reaction is completed to obtain a modifier;
[0053] (2) Add 72 mL of isobutanol and 12 mL of deionized water to the reactor, add hydrochloric acid to adjust the pH to 5, then add 0.2 g of the modifier, stir and mix at 50° C. for 5.5 h to obtain the hydrolyzed modifier, then add 1.9 g of silica, continue to heat to 65° C., set the stirring condition to 450 r / min, stir and react for 4.5 h to obtain modified silica I.
[0054] Preparation Example 2
[0055] The preparation steps of modified silica II are the same as those of Preparation Example 1, except that 1.4 g of silica is added in step (2).
[0056] Preparation Example 3
[0057] The preparation steps of modified silica III are the same as those of Preparation Example 1, except that 2.6 g of silica is added in step (2).
[0058] Preparation Example 4
[0059] The preparation steps of modified organosiloxane I are as follows: add 1.2g of hydroxypolydimethylsiloxane into a reactor, add 2g of thermoplastic copolymer TSM, stir well, add 0.12g of diphenylbutyl carbamate, and obtain modified organosiloxane I at 85°C.
[0060] Preparation Example 5
[0061] The preparation steps of modified organosiloxane II are the same as those of Preparation Example 4, except that 0.4 g of hydroxypolydimethylsiloxane is added.
[0062] Preparation Example 6
[0063] The preparation steps of modified organosiloxane II are the same as those of Preparation Example 4, except that 2.2 g of hydroxypolydimethylsiloxane is added.
[0064] Example 1
[0065] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0066] Wherein, the thickness of the foam glue is 8.5mm;
[0067] The preparation steps of the flame retardant double-sided adhesive are as follows: by weight, 35 parts of amino-containing acrylic polymer resin, 17.5 parts of chloroprene rubber, 6.5 parts of hydrogenated rosin and 10 parts of silicone flame retardant are added into a reactor, 3 parts of modified silicon dioxide I are added and mixed evenly, and then 6.5 parts of isocyanate are added and mixed thoroughly to obtain the flame retardant double-sided adhesive;
[0068] The preparation steps of the foamed silica gel are as follows: by weight, 75 parts of modified organosiloxane I are added into a reactor, and then 22.5 parts of fumed silica and 35 parts of organosilicon flame retardant are added into the container, stirred at 75° C. for 1.2 hours, and then stirred under vacuum for 15 minutes, the temperature is lowered to 10.5° C., and then 0.51 parts of platinum catalyst are added and mixed evenly, and then 7 parts of hydrogenated silicone oil are added and stirred for 20 minutes to obtain the foamed silica gel;
[0069] The method for preparing the collision-resistant and waterproof foam adhesive of this embodiment comprises the following steps:
[0070] The flame retardant double-sided adhesive is coated on the release layer to form the first flame retardant double-sided adhesive layer, with a dry weight of 36.3g / m 2 , and then a cotton paper layer is attached on the first flame retardant double-sided adhesive layer, and then a flame retardant double-sided adhesive is applied on the cotton paper layer to form a second flame retardant double-sided adhesive layer, with a dry weight of 36.3g / m 2 Then, a foamed silica gel is coated on the second flame retardant double-sided adhesive layer to form a foamed silica gel layer, and then the foamed silica gel layer is cured at 35° C. to obtain the collision-resistant and waterproof foam adhesive.
[0071] Example 2
[0072] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0073] Wherein, the thickness of the foam glue is 2mm;
[0074] The preparation steps of the flame retardant double-sided adhesive are as follows: by weight, 20 parts of amino-containing acrylic polymer resin, 10 parts of chloroprene rubber, 3 parts of hydrogenated rosin and 2 parts of silicone flame retardant are added into a reactor, 1 part of modified silicon dioxide I is added and mixed evenly, and then 3 parts of isocyanate are added and mixed thoroughly to obtain the flame retardant double-sided adhesive;
[0075] The preparation steps of the foamed silica gel are the same as those in Example 1;
[0076] The method for preparing the collision-resistant and waterproof foam adhesive of this embodiment comprises the following steps:
[0077] The flame retardant double-sided adhesive is coated on the release layer to form the first flame retardant double-sided adhesive layer, with a dry weight of 35g / m 2Then, a cotton paper layer is laminated on the first flame retardant double-sided adhesive layer, and then a flame retardant double-sided adhesive is coated on the cotton paper layer to form a second flame retardant double-sided adhesive layer, with a dry weight of 35g / m 2 Then, a foamed silica gel is coated on the second flame retardant double-sided adhesive layer to form a foamed silica gel layer, and then the foamed silica gel layer is cured at 20° C. to obtain the collision-resistant and waterproof foam adhesive.
[0078] Example 3
[0079] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0080] Wherein, the thickness of the foam glue is 15mm;
[0081] The preparation steps of the flame retardant double-sided adhesive are as follows: by weight, 50 parts of amino-containing acrylic polymer resin, 25 parts of chloroprene rubber, 15 parts of hydrogenated rosin and 18 parts of silicone flame retardant are added into a reactor, 5 parts of modified silicon dioxide I are added and mixed evenly, and then 5 parts of isocyanate are added and mixed thoroughly to obtain the flame retardant double-sided adhesive;
[0082] The preparation steps of the foamed silica gel are the same as those in Example 1;
[0083] The method for preparing the collision-resistant and waterproof foam adhesive of this embodiment comprises the following steps:
[0084] The flame retardant double-sided adhesive is coated on the release layer to form the first flame retardant double-sided adhesive layer, with a dry weight of 37.5g / m 2 , and then a cotton paper layer is attached on the first flame retardant double-sided adhesive layer, and then a flame retardant double-sided adhesive is applied on the cotton paper layer to form a second flame retardant double-sided adhesive layer, with a dry weight of 37.5g / m 2 Then, a foamed silica gel is coated on the second flame retardant double-sided adhesive layer to form a foamed silica gel layer, and then cured at 50° C. to obtain the collision-resistant and waterproof foam adhesive.
[0085] Example 4
[0086] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0087] Wherein, the thickness of the foam glue is 8.5mm;
[0088] The preparation steps of the flame retardant double-sided adhesive are the same as those in Example 1;
[0089] The preparation steps of the foamed silica gel are as follows: by weight, 50 parts of modified organosiloxane I are added into a reactor, and then 10 parts of fumed silica and 20 parts of organosilicon flame retardant are added into the container, stirred at 60° C. for 1.6 hours, and then stirred under vacuum for 5 minutes, the temperature is lowered to 6° C., and then 0.01 parts of platinum catalyst are added and mixed evenly, and then 6 parts of hydrogenated silicone oil are added and stirred for 10 minutes to obtain the foamed silica gel;
[0090] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0091] Example 5
[0092] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0093] Wherein, the thickness of the foam glue is 8.5mm;
[0094] The preparation steps of the flame retardant double-sided adhesive are the same as those in Example 1;
[0095] The preparation steps of the foamed silica gel are as follows: by weight, 100 parts of modified organosiloxane I are added into a reactor, 35 parts of fumed silica and 50 parts of organosilicon flame retardant are added into the container, stirred at 90° C. for 0.8 h, stirred under vacuum for 25 min, the temperature was lowered to 15° C., 10 parts of platinum catalyst were added and mixed evenly, 8 parts of hydrogenated silicone oil were added, and stirred for 30 min to obtain the foamed silica gel;
[0096] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0097] Example 6
[0098] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0099] Wherein, the thickness of the foam glue is 8.5mm;
[0100] The preparation steps of the flame retardant double-sided adhesive are the same as those of Example 1, except that modified silicon dioxide II is used in equal amounts to replace modified silicon dioxide I;
[0101] The preparation steps of the foamed silica gel are the same as those in Example 1;
[0102] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0103] Example 7
[0104] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0105] Wherein, the thickness of the foam glue is 8.5mm;
[0106] The preparation steps of the flame retardant double-sided adhesive are the same as those of Example 1, except that modified silicon dioxide III is used to replace modified silicon dioxide I in equal amounts;
[0107] The preparation steps of the foamed silica gel are the same as those in Example 1;
[0108] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0109] Example 8
[0110] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0111] Wherein, the thickness of the foam glue is 8.5mm;
[0112] The preparation steps of the flame retardant double-sided adhesive are the same as those of Example 1, except that an equal amount of silicon dioxide is used to replace the modified silicon dioxide I;
[0113] The preparation steps of the foamed silica gel are the same as those in Example 1;
[0114] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0115] Example 9
[0116] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0117] Wherein, the thickness of the foam glue is 8.5mm;
[0118] The preparation steps of the flame retardant double-sided adhesive are the same as those in Example 1;
[0119] The steps for preparing the foamed silica gel are the same as those of Example 1, except that the modified organosiloxane I is replaced by an equal amount of modified organosiloxane II;
[0120] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0121] Example 10
[0122] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0123] Wherein, the thickness of the foam glue is 8.5mm;
[0124] The preparation steps of the flame retardant double-sided adhesive are the same as those in Example 1;
[0125] The steps for preparing the foamed silica gel are the same as those of Example 1, except that the modified organosiloxane III is used to replace the modified organosiloxane I in equal amounts;
[0126] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0127] Embodiment 11
[0128] A collision-resistant and waterproof foam adhesive, the foam adhesive sequentially comprising a composite release layer, a first flame-retardant double-sided adhesive layer, a cotton paper layer, a second flame-retardant double-sided adhesive layer and a foamed silica gel layer;
[0129] Wherein, the thickness of the foam glue is 8.5mm;
[0130] The preparation steps of the flame retardant double-sided adhesive are the same as those in Example 1;
[0131] The steps for preparing the foamed silica gel are the same as those of Example 1, except that an equal amount of hydroxy polydimethylsiloxane is used to replace the modified organosiloxane I;
[0132] The preparation method of the collision-resistant and waterproof foam adhesive in this embodiment is the same as that in Embodiment 1.
[0133] Performance Testing:
[0134] The collision-resistant and waterproof foam adhesive prepared in the above embodiments was subjected to the following performance tests, and the test results are shown in Table 1:
[0135] (1) Flame retardant performance test: The flame retardant grade of foam glue is tested in accordance with the standard GB / T2408-2021. The flame retardant grades include HB, V-2, V-1 and V-0. HB grade is the lowest grade and is suitable for occasions with lower flame retardant requirements. The flame retardant performance of V-2, V-1 and V-0 grades increases step by step;
[0136] (2) Impact resistance test: The drop hammer impact test method was used, with the impact energy set at 15 J and the speed at 2.7 m / s. The energy absorption rate of the foam adhesive was used to represent the impact resistance of the foam adhesive. The higher the absorption rate, the better the impact resistance.
[0137] (3) Water resistance test: The foam adhesive prepared in each example was immersed in 50° C. water for 24 hours and then the state of the foam adhesive was observed to see if it fell off.
[0138] Table 1
[0139] project Flame retardant grade Absorption rate / % Water resistance / whether it falls off Example 1 V-0 56.8 no Example 2 V-0 55.9 no Example 3 V-0 54.5 no Example 4 V-0 52.1 no Example 5 V-0 52.7 no Example 6 V-0 50.4 no Example 7 V-1 48.5 no Example 8 V-1 48.1 yes Example 9 V-0 47.3 yes Example 10 V-0 48 yes Embodiment 11 V-0 46.7 yes
[0140] As can be seen from Table 1, the foam adhesive prepared in Examples 1 to 5 of the present invention is a high-performance foam adhesive with excellent collision resistance, good flame retardant effect and waterproofness, and the flame retardant grade is V-0, with excellent impact resistance and collision resistance, and can be used for a long time while maintaining soft elasticity, and has good water resistance and excellent comprehensive performance. The flame retardant double-sided adhesive used in Examples 6, 7 and 8 changed the preparation conditions of modified silica during the preparation process, which affected the compatibility of modified silica in the system, resulting in negative enhancement, fluctuations in various performance tests, and significantly affected the performance of the combustion-supporting component, resulting in a weakening of the synergistic flame retardant effect. The preparation conditions of the modified organic siloxane were changed during the preparation of the foamed silica gel, which affected the interfacial interaction between the thermoplastic polymer and the organic siloxane and affected the stress transfer effect. Compared with Examples 1 to 5, the impact resistance of the foamed silica gel layer preferably provided by the present invention was significantly improved, especially compared with the unmodified organic siloxane, indicating that its compressive effect and impact toughness were improved; the water resistance test results also showed that the foamed silica gel preferably prepared by the present invention avoided the influence of agglomeration and accumulation caused by the expansion of the thermoplastic copolymer on the interfacial interaction in the modified organic siloxane structure, reduced its influence on the hydrophobicity of the foamed silica gel, and synergistically improved the chemical stability of the foam glue.
[0141] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A collision-resistant and waterproof foam adhesive, characterized in that: The foam adhesive comprises a composite release layer, a first flame retardant double-sided adhesive layer, a tissue paper layer, a second flame retardant double-sided adhesive layer and a foamed silica gel layer in sequence; Wherein, the thickness of the foam glue is 2 to 15 mm.
2. A method for preparing the collision-resistant and waterproof foam adhesive according to claim 1, characterized in that: The process comprises the following steps: coating the release layer with a flame retardant double-sided adhesive to form a first flame retardant double-sided adhesive layer, the dry weight of which is 35 to 37.5 g / m 2 , and then a cotton paper layer is attached on the first flame retardant double-sided adhesive layer, and then a flame retardant double-sided adhesive is applied on the cotton paper layer to form a second flame retardant double-sided adhesive layer, the dry weight of which is 35-37.5g / m 2 Then, a foamed silica gel is coated on the second flame retardant double-sided adhesive layer to form a foamed silica gel layer, and the foamed silica gel layer is cured at 20-50° C. to obtain the collision-resistant and waterproof foam adhesive.
3. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 2, characterized in that: The flame retardant double-sided adhesive comprises the following raw materials in parts by weight: 20 to 50 parts of acrylic prepolymer, 10 to 25 parts of adhesive, 3 to 10 parts of tackifying resin, 2 to 18 parts of first flame retardant, 1 to 5 parts of modified silicon dioxide and 3 to 5 parts of isocyanate curing agent.
4. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 3, characterized in that: The preparation steps of the modified silicon dioxide are as follows: (1) Adding a composite silane coupling agent into a reactor, stirring and heating to 110-130° C. under an inert atmosphere, reacting for 4-7 hours, cooling to room temperature after the reaction is completed, and obtaining a modifier; (2) Take another reactor and add solvent, adjust the pH to 4-6, then add modifier, stir and mix at 40-60°C for 3-8h to obtain hydrolyzed modifier, then add silica, continue to heat to 60-70°C, set stirring conditions to 400-500 r / min, stir and react for 4-5h to obtain modified silica.
5. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 4, characterized in that: The mass ratio of the modifier to silicon dioxide is 1:(7-12).
6. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 3, characterized in that: The mass ratio of the first flame retardant to the modified silicon dioxide is 1:(0.2-0.5).
7. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 3, characterized in that: The preparation steps of the flame retardant double-sided adhesive are as follows: adding acrylic prepolymer, adhesive, tackifying resin and first flame retardant into a reactor, adding modified silicon dioxide and mixing evenly, then adding isocyanate curing agent and mixing thoroughly to obtain the flame retardant double-sided adhesive.
8. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 2, characterized in that: The foamed silica gel comprises the following raw materials in parts by weight: 50-100 parts of modified organic siloxane, 10-35 parts of fumed silica, 0.6-2 parts of methyl hydrogenated silicone oil, 20-50 parts of a second flame retardant, 0.01-1.0 parts of a catalyst and 6-8 parts of hydrogenated silicone oil.
9. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 8, characterized in that: The preparation steps of the modified organosiloxane are as follows: adding the organosiloxane into a reactor, adding the thermoplastic copolymer, stirring evenly, adding the curing agent, stirring and reacting at 80-90° C. for 1-3 hours to obtain the modified organosiloxane.
10. The method for preparing the collision-resistant and waterproof foam adhesive according to claim 8, characterized in that: The preparation steps of the foamed silica gel are as follows: adding modified organic siloxane into a reactor, then adding fumed silica and a second flame retardant into a container, stirring at 60 to 90° C. for 0.8 to 1.6 hours, then stirring under vacuum for 5 to 25 minutes, lowering the temperature to 6 to 15° C., then adding a catalyst and mixing evenly, then adding hydrogenated silicone oil, stirring for 10 to 30 minutes, and obtaining the foamed silica gel.