Epoxy adhesive, preparation method thereof and application of epoxy adhesive in rail transit floor

Through the two-component system design epoxy adhesive, combined with toughening agent and modified polyetheramine curing agent, the problems of insufficient bonding strength and long curing time in rail transit floors are solved, and efficient and easy-to-operate adhesives are achieved The connection effect is improved and the stability and safety of the floor are improved.

CN118931449AInactive Publication Date: 2024-11-12CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411162078.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the application of rail transit floors, existing epoxy adhesives have problems such as insufficient bonding strength, long curing time and difficulty in disassembly, which is difficult to meet the special needs of rail transit floor materials, affecting safety and service life.

Method used

The epoxy adhesive designed with a two-component system is used to reasonably prepare components A and B, and add toughening agents and modified polyetheramine curing agents to form adhesive materials with good stability and controllability. It can cure quickly at room temperature, improve bond strength and durability, and is easy to disassemble.

Benefits of technology

It realizes strong bonding on rail transit floors, improves bonding strength and durability, reduces operating costs, ensures the stability and safety of the floors, and reduces the negative impact on the environment and human health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931449A_ABST
    Figure CN118931449A_ABST
Patent Text Reader

Abstract

The invention relates to an epoxy adhesive, a preparation method thereof and application of the epoxy adhesive in a rail transit floor. The invention belongs to the field of adhesives. The problems that an existing epoxy adhesive is long in curing time, insufficient in bonding strength, poor in flame retardance and the like are solved. According to the invention, through the design of a two-component system, the adhesive has better stability and controllability, the bonding strength and durability are improved, the adhesive can be cured at room temperature, the experiment is simple, the operation is convenient, the industrial production is facilitated, and through the selection and proportion of all the components, the adhesive has excellent performance in the aspects of water resistance and durability, and has good application prospects. The adhesive can be used for the powerful bonding of various types of wood boards and floors, can meet the special requirements of floor materials of rail transit vehicles, and ensures the stability and safety of the floors of the rail transit vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adhesives, and in particular relates to an epoxy adhesive and a preparation method thereof and application thereof in rail transit floors. Background Art

[0002] Epoxy adhesives are widely used and can be used to bond various metals and alloys, non-metallic materials such as ceramics, glass, wood, cardboard, plastic, concrete, stone, bamboo, etc., and can also be used to bond metals to non-metallic materials. Epoxy resin itself is a linear thermoplastic substance, and its fracture energy and fracture toughness are much smaller than other plastics. After adding curing agent, the cured product has a three-dimensional network structure, which is hard and brittle in nature. When epoxy resin is heated, cured and cooled to form a cured product, the internal stress generated by shrinkage will cause cracks inside the cured product, making the cured product not resistant to heat shock.

[0003] With the rapid development of the rail transit industry, the demand for bonding floor materials in trains is also increasing. Traditional floor material bonding mostly relies on mechanical connection or simple glue bonding, but these methods often have problems such as low bonding strength, short service life, high temperature resistance, and easy aging. Epoxy adhesives, as a high-performance adhesive material, are widely used in the field of rail transit. However, epoxy adhesives in the prior art often have the characteristics of high hardness, strong brittleness, insufficient toughness, and difficulty in removal, which makes it difficult to meet the special needs of floor materials for rail transit. These problems seriously affect the safety and service life of rail transit floors. Therefore, the development of an epoxy adhesive with excellent bonding performance, outstanding toughness, good water resistance, easy operation, fast curing, and easy disassembly will play an important role in improving the bonding quality of rail transit floors. Summary of the invention

[0004] In view of the above problems, the present invention provides an epoxy adhesive and a preparation method thereof, aiming to solve the shortcomings of existing epoxy adhesives such as long curing time, insufficient bonding strength and difficult disassembly. The present invention provides an epoxy adhesive and a preparation method and application thereof. Through a two-component system design, the adhesive has better stability and controllability, and improves bonding strength and durability.

[0005] The technical solution of the present invention is as follows:

[0006] One of the purposes of the present invention is to provide an epoxy adhesive, wherein the epoxy adhesive is composed of a component A and a component B which are separately packaged, wherein the component A is composed of the following components in parts by mass:

[0007] 50-85 parts of epoxy resin, 3-5 parts of active diluent, 0.2-0.7 parts of coupling agent, 1.1-1.7 parts of first auxiliary agent, 10-30 parts of filler, 8-20 parts of toughening agent;

[0008] The B component is composed of the following ingredients in parts by mass:

[0009] 0 to 20 parts of polyamide curing agent, 0 to 55 parts of polyetheramine curing agent, 0.3 to 1.5 parts of second auxiliary agent, 15 to 72 parts of other amine curing agent, 0 to 10 parts of solvent, and 0 to 10 parts of accelerator.

[0010] It is further defined that the mass ratio of component A to component B is 100:20-30.

[0011] It is further defined that the epoxy resin is at least one of bisphenol A epoxy resin, bisphenol F epoxy resin or bisphenol S epoxy resin.

[0012] It is further defined that the active diluent is at least one of alkyl glycidyl ether, neopentyl glycol diglycidyl ether, phenyl glycidyl ether, polyphenol glycidyl ether or ethylene glycol diglycidyl ether.

[0013] It is further defined that the coupling agent is at least one of γ-glycidyloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane or 3-glycidyloxypropyltriethoxysilane.

[0014] It is further defined that the filler is at least one of titanium dioxide, talc, ammonium polyphosphate, aluminum hydroxide, phosphazene or mica powder.

[0015] It is further defined that the toughening agent is carboxyl-terminated nitrile rubber, epoxy-terminated liquid nitrile rubber or hydroxyl-terminated liquid nitrile rubber.

[0016] It is further defined that the first auxiliary agent is at least one of a dispersant, a defoamer, a leveling agent or an antioxidant.

[0017] It is further defined that the second auxiliary agent is at least one of a dispersant or a defoaming agent.

[0018] It is further defined that the dispersant is a high molecular polymer; the defoaming agent is a modified organic silicon compound; the leveling agent is a polyether modified organic silicon compound; and the antioxidant is an antioxidant.

[0019] It is further defined that the high molecular polymer is at least one of KYC-918, BYK163, BYK-190, BYK405 or KMT3331; the modified silicone compound is at least one of AKN-3801, KMT-6015, BYK-057 or BYK-088; the polyether modified silicone compound is at least one of AKN-1050, KMT-5251, KMT-5502, BYK-333 or BYK-346; and the antioxidant is at least one of antioxidant 264, antioxidant 1010 or antioxidant 1076.

[0020] It is further defined that the polyamide curing agent is at least one of curing agents YD-8140, YD-8216, YD8200N, YD-8125A or YD-8115.

[0021] It is further defined that the polyetheramine curing agent is at least one of polyetheramine D230, polyetheramine D400, polyetheramine D2000 or modified polyetheramine.

[0022] In a further embodiment, the modified polyetheramine is a polyetheramine modified with diethylene glycol di(3-aminopropyl) ether (DEGBAE).

[0023] It is further defined that the other amine curing agent is at least one of cardanol-modified phenolic amine, N-aminoethylpiperazine, diethylenetriamine, triethylenetetramine or tetraethylenepentamine.

[0024] It is further defined that the solvent is at least one of benzyl alcohol or acetophenone.

[0025] It is further defined that the accelerator is at least one of DMP-30 or 3-dimethylaminopropylamine.

[0026] A second object of the present invention is to provide a method for preparing an epoxy adhesive, wherein:

[0027] Preparation of component A: Mix epoxy resin, diluent, coupling agent, first auxiliary agent and toughening agent, add filler, perform vacuum dispersion and degassing, and then pack;

[0028] Preparation of component B: Mix and disperse the polyamide curing agent, polyetheramine curing agent, second auxiliary agent, other amine curing agent, solvent and accelerator in vacuum and then pack them;

[0029] Preparation of epoxy adhesive: When using, mix component A and component B evenly to obtain epoxy adhesive.

[0030] A third object of the present invention is to provide an application of the above-mentioned epoxy adhesive in rail transit floors.

[0031] Compared with the prior art, the specific advantages of the present invention are as follows:

[0032] (1) The epoxy adhesive of the present invention adopts a two-component system design, which makes the adhesive have better stability and controllability, improves the bonding strength and durability, and is suitable for various types of PVC floors, including smooth floors, non-smooth floors, and floors with mesh cloth. It can achieve strong bonding between floors, can meet the special needs of rail transit floor materials, and ensure the stability and safety of rail transit floors.

[0033] (2) The toughening agents added in the present invention all have active groups, can participate in the curing reaction, increase toughness without increasing hardness, and will not precipitate after curing. The homemade modified polyetheramine curing agent used in the present invention contains a flexible segment, which has the advantages of low toxicity, low volatility and low odor. The cured epoxy adhesive can not only enhance toughness, but also show good flexibility.

[0034] (3) The epoxy adhesive of the present invention can be cured at room temperature, the experiment is simple, the operation is convenient, and no additional heating is required, which reduces the cost and improves the efficiency, and can greatly shorten the maintenance and renovation cycle of rail transit floors.

[0035] (4) The present invention does not contain any highly toxic substances such as formaldehyde, benzene, toluene and xylene during the raw material selection and preparation process, ensuring that while meeting conventional usage requirements, the negative impact on the environment and human health is minimized. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is the modified polyetheramine in Example 1 1 H-NMR;

[0037] Figure 2 This is the infrared spectrum of the modified polyetheramine in Example 1. DETAILED DESCRIPTION

[0038] The present invention provides a method for preparing an epoxy adhesive, which is achieved by the following steps:

[0039] Preparation of component A: Mix epoxy resin (50-85 parts), active diluent (3-5 parts), coupling agent (0.2-0.7 parts), first auxiliary agent (1.1-1.7 parts) and toughening agent (8-20 parts) under vacuum conditions, add filler (10-30 parts), disperse evenly under vacuum at room temperature, degas, and package after degassing;

[0040] Preparation of component B: polyamide curing agent (0-20 parts), polyetheramine curing agent (0-55 parts), second auxiliary agent (0.3-1.5 parts), other amine curing agent (15-72 parts), solvent (0-10 parts) and accelerator (0-10 parts) are mixed and dispersed in vacuum at room temperature and then packaged;

[0041] Preparation of epoxy adhesive: Component A (100 parts) and component B (20-30 parts) are mixed evenly to obtain epoxy adhesive.

[0042] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0043] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0044] The terms "comprising," "including," "having," "containing," or any other variations thereof, as used in the following examples, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.

[0045] When equivalent, concentration or other value or parameter is represented by the range limited by range, preferred range or a series of upper preferred value and lower preferred value, this should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the scope is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, range limitation can be combined and / or interchanged, if these ranges are not otherwise stated, include all sub-ranges contained therein.

[0046] The "one embodiment" or "embodiment" of the present invention refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.

[0047] The bisphenol A epoxy resin E51 used in the following examples was ordered from Nantong Xingchen Synthetic Materials Co., Ltd.; the carboxyl-terminated nitrile rubber was ordered from Olilon (Jining) Chemical Co., Ltd.

[0048] Embodiment 1:

[0049] Preparation of component A: bisphenol A epoxy resin E51 (64.4 parts), AGE diluent (4.6 parts), γ-glycidyloxypropyl trimethoxysilane (0.4 parts), dispersant KYC-918 (0.3 parts), leveling agent AKN-1050 (0.2 parts), antioxidant 1076 (0.2 parts), defoamer AKN-3801 (0.8 parts) and carboxyl-terminated nitrile rubber (18.4 parts) were added to a reactor at room temperature, and the mixture was stirred and dispersed under vacuum at a stirring speed of 40 rpm and a dispersion speed of 400 rpm. After stirring evenly, titanium dioxide (3.7 parts), talcum powder (6.9 parts) and fumed silica (1.0 parts) were added, and the dispersion speed was increased to 650 rpm. The mixture was dispersed for 1.5 hours and defoamed for 30 minutes to obtain component A.

[0050] The structural formula of modified polyetheramine is:

[0051] Preparation of component B: Add polyamide curing agent YD-8140 (16.3 parts), modified polyetheramine curing agent (9.9 parts), defoamer AKN-3801 (0.1 parts), polyetheramine D2000 (38.1 parts), tetraethylenepentamine (27.2 parts), benzyl alcohol (4.9 parts) and accelerator DMP-30 (3.3 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 30 rpm, the dispersion speed is 400 rpm, and degassing treatment is performed for 30 minutes after 1 hour to obtain component B;

[0052] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0053] Embodiment 2:

[0054] Preparation of component A: bisphenol A epoxy resin E51 (82.4 parts), AGE diluent (5.9 parts), γ-glycidyloxypropyl trimethoxysilane (0.5 parts), dispersant KYC-918 (0.4 parts), leveling agent AKN-1050 (0.2 parts), antioxidant 1076 (0.2 parts), defoamer AKN-3801 (0.8 parts) and carboxyl-terminated nitrile rubber (8.4 parts) were added to a reactor at room temperature, and the mixture was stirred and dispersed under vacuum at a speed of 40 rpm and a dispersion speed of 400 rpm. After stirring evenly, titanium dioxide (4.7 parts), talcum powder (23.6 parts) and fumed silica (1.2 parts) were added, and the dispersion speed was increased to 650 rpm. The mixture was dispersed for 1.5 hours and defoamed for 30 minutes to obtain component A.

[0055] Preparation of component B: add cardanol modified phenolic amine (53.7 parts), N-aminoethylpiperazine (17.5 parts), defoamer AKN-3801 (0.3 parts), tetraethylenepentamine (17.5 parts), γ-glycidyloxypropyltrimethoxysilane (0.5 parts), 3-dimethylaminopropylamine (1.9 parts) and accelerator DMP-30 (8.1 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 30 rpm, the dispersion speed is 400 rpm, and degassing treatment is performed for 30 minutes after 1 hour to obtain component B;

[0056] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0057] Embodiment 3:

[0058] Preparation of component A: bisphenol A epoxy resin E51 (67.5 parts), AGE diluent (3.5 parts), γ-glycidyloxypropyl trimethoxysilane (0.4 parts), dispersant KYC-918 (0.3 parts), leveling agent AKN-1050 (0.2 parts), antioxidant 1076 (0.2 parts), defoamer AKN-3801 (0.8 parts) and carboxyl-terminated nitrile rubber (15.6 parts) were added to a reactor at room temperature, and the mixture was stirred and dispersed at a speed of 35 rpm and a dispersion speed of 400 rpm. After stirring evenly, titanium dioxide (3.7 parts), talc (4.9 parts), aluminum hydroxide (11.3 parts) and fumed silica (1.2 parts) were added, and the dispersion speed was increased to 650 rpm. The mixture was dispersed for 2 hours and defoamed for 30 minutes to obtain component A.

[0059] Preparation of component B: Add polyamide curing agent YD-8125A (19.9 parts), polyetheramine D2000 (46.4 parts), tetraethylenepentamine (33.1 parts) and γ-aminopropyltriethoxysilane (0.4 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 35 rpm, the dispersion speed is 400 rpm, and degassing treatment is performed for 30 minutes after 1 hour to obtain component B;

[0060] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0061] Embodiment 4:

[0062] Preparation of component A: bisphenol A epoxy resin E51 (56.5 parts), AGE diluent (4.0 parts), γ-glycidyloxypropyl trimethoxysilane (0.3 parts), dispersant KYC-918 (0.2 parts), leveling agent AKN-1050 (0.2 parts), antioxidant 1076 (0.2 parts), defoamer AKN-3801 (0.7 parts) and carboxyl-terminated nitrile rubber (16.1 parts) were added to a reactor at room temperature, and the mixture was stirred and dispersed under vacuum at a stirring speed of 45 rpm and a dispersion speed of 400 rpm. After stirring evenly, titanium dioxide (3.2 parts), phosphazene (17.6 parts) and fumed silica (0.8 parts) were added, and the dispersion speed was increased to 650 rpm. The mixture was dispersed for 2 hours and defoamed for 30 minutes to obtain component A.

[0063] The modified polyetheramine is the same as in Example 1;

[0064] Preparation of component B: Add polyamide curing agent YD-8140 (15.5 parts), modified polyetheramine curing agent (9.4 parts), γ-aminopropyltriethoxysilane (0.3 parts), polyetheramine D2000 (36.3 parts), tetraethylenepentamine (25.9 parts), benzyl alcohol (9.4 parts) and accelerator DMP-30 (3.1 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 30 rpm, the dispersion speed is 400 rpm, and degassing treatment is performed for 30 minutes after 1 hour to obtain component B;

[0065] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0066] Embodiment 5:

[0067] Preparation of component A: bisphenol A epoxy resin E51 (54.1 parts), AGE diluent (3.9 parts), γ-glycidyloxypropyl trimethoxysilane (0.3 parts), dispersant KYC-918 (0.2 parts), leveling agent AKN-1050 (0.2 parts), antioxidant 1076 (0.2 parts), defoamer KMT-6015 (0.7 parts) and carboxyl-terminated nitrile rubber (15.5 parts) were added to a reactor at room temperature, and the mixture was stirred and dispersed under vacuum at a stirring speed of 35 rpm and a dispersion speed of 400 rpm. After stirring evenly, titanium dioxide (3.1 parts), ammonium polyphosphate (5.8 parts), phosphazene (15.3 parts) and fumed silica (0.8 parts) were added, and the dispersion speed was increased to 650 rpm. The mixture was dispersed for 2 hours and defoamed for 30 minutes to obtain component A.

[0068] The modified polyetheramine is the same as in Example 1;

[0069] Preparation of component B: Add polyamide curing agent YD-8200N (9.4 parts), polyetheramine D230 (10.9 parts), polyamide curing agent (15.5 parts), γ-aminopropyltriethoxysilane (0.3 parts), triethylenetetramine (24.1 parts), benzyl alcohol (9.4 parts) and accelerator DMP-30 (5.0 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 20-50rpm, the dispersion speed is 400rpm, and degassing treatment is performed for 30min after 1h to obtain component B;

[0070] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0071] Embodiment 6:

[0072] Preparation of component A: bisphenol A epoxy resin E51 (64.4 parts), AGE diluent (4.6 parts), γ-glycidyloxypropyl trimethoxysilane (0.4 parts), dispersant KYC-918 (0.3 parts), leveling agent AKN-1050 (0.2 parts), antioxidant 1076 (0.2 parts), defoamer AKN-3801 (0.8 parts) and carboxyl-terminated nitrile rubber (18.4 parts) were added to a reactor at room temperature, and the mixture was stirred and dispersed under vacuum at a stirring speed of 45 rpm and a dispersion speed of 400 rpm. After stirring evenly, titanium dioxide (3.2 parts), talcum powder (6.9 parts) and fumed silica (1.5 parts) were added, and the dispersion speed was increased to 650 rpm. The mixture was dispersed for 1 hour and defoamed for 30 minutes to obtain component A.

[0073] The modified polyetheramine is the same as in Example 1;

[0074] Component B was prepared in the same manner as in Example 1;

[0075] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0076] Embodiment 7:

[0077] Component A was prepared in the same manner as in Example 1;

[0078] The modified polyetheramine is the same as in Example 1;

[0079] Preparation of component B: Add polyamide curing agent YD-8140 (16.3 parts), modified polyetheramine curing agent (9.9 parts), defoamer AKN-3801 (0.1 parts), polyetheramine D2000 (38.1 parts), tetraethylenepentamine (27.2 parts), benzyl alcohol (4.9 parts) and accelerator DMP-30 (6.3 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 20-50rpm, the dispersion speed is 400rpm, and degassing treatment is performed for 30min after 1h to obtain component B;

[0080] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0081] Comparative Example 1:

[0082] Component A was prepared in the same manner as in Example 4;

[0083] The modified polyetheramine is the same as in Example 1;

[0084] Component B was prepared in the same manner as in Example 4;

[0085] Preparation of epoxy adhesive: Component A (100 parts) and component B (15 parts) were mixed evenly to obtain epoxy adhesive.

[0086] Comparative Example 2:

[0087] Component A was prepared in the same manner as in Example 4;

[0088] The modified polyetheramine is the same as in Example 1;

[0089] Preparation of component B: Add polyamide curing agent YD-8115 (15.5 parts), modified polyetheramine curing agent (4.7 parts), γ-aminopropyltriethoxysilane (0.3 parts), polyetheramine D2000 (36.3 parts), tetraethylenepentamine (25.9 parts), benzyl alcohol (9.4 parts) and accelerator DMP-30 (3.1 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 20-50rpm, the dispersion speed is 400rpm, and degassing treatment is performed for 30min after 1h to obtain component B;

[0090] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0091] Comparative Example 3:

[0092] Component A was prepared in the same manner as in Example 4;

[0093] Preparation of component B: Add polyamide curing agent YD-8115 (15.5 parts), γ-aminopropyltriethoxysilane (0.3 parts), polyetheramine D2000 (36.3 parts), tetraethylenepentamine (25.9 parts), benzyl alcohol (9.4 parts) and accelerator DMP-30 (3.1 parts) into a reaction kettle under vacuum at room temperature, evacuate and stir to disperse, the stirring speed is 20-50rpm, the dispersion speed is 400rpm, and degassing treatment is performed for 30min after 1h to obtain component B;

[0094] Preparation of epoxy adhesive: Component A (100 parts) and component B (20 parts) were mixed evenly to obtain epoxy adhesive.

[0095] Performance Testing

[0096] The following performance tests were performed on the epoxy adhesives for floor bonding prepared in the above-mentioned embodiments 1, 2, 3, 4, 5, 6 and 7 and the epoxy adhesives for floor bonding prepared in the comparative examples 1, 2 and 3:

[0097] Working time: Determined according to GB / T 7123.1-2015 Working time of multi-component adhesives.

[0098] Shear strength: Determined according to GB / T 7124-2008 "Determination of tensile shear strength of adhesives (rigid material to rigid material)".

[0099] Peel strength / floor cloth-aluminum alloy: measured in accordance with GB / T 2790-1995 "Adhesive 180° glass strength test method - Flexible material to rigid material".

[0100] The epoxy adhesives for floor bonding prepared in the above examples and comparative examples were subjected to performance tests, and the following data were obtained, as shown in Table 1:

[0101] Table 1 Performance test table of epoxy adhesive for floor bonding in embodiments and comparative examples

[0102]

[0103] Supplementary explanation for Table 1: Curing conditions: standing at 23±2°C for 7 days.

[0104] The data in Table 1 prove that the present invention improves the curing speed and toughness of the adhesive by adjusting the curing agent ratio and the amount of the modified polyetheramine curing agent added. Generally speaking, when a toughening agent is added, the toughness is enhanced and the shear strength is greatly reduced. Therefore, the present invention greatly enhances the toughness of the epoxy adhesive while ensuring the shear strength by adding a small amount of modified polyetheramine curing agent. It can be seen from the peeling test specimen that the adhesive on the torn specimen has no cracks, and the floor with good toughness is easy to disassemble.

[0105] In addition, the present invention achieves synergistic effect by compounding modified polyetheramine curing agent and polyamide curing agent to epoxy resin curing. First, structurally speaking, the flexible polyether segment in the modified polyetheramine makes the cured product have good flexibility and impact resistance. On this basis, it can form a chemical structure complementary with the amide bond on the polyamide, provide higher strength and hardness, and make the cured product reach a better balance in flexibility and strength. Secondly, in terms of reaction activity, the large amount of heat release of the curing reaction of the modified polyetheramine promotes the initial stage of the curing process, shortens the time of initial curing, and is conducive to the next stage of the process in the actual construction process. At the same time, the polyamide continues to play a role in the late stage of curing to ensure that the curing reaction is fully carried out. The compounded curing agent can maintain a relatively stable reaction rate throughout the curing process, avoiding the problem of too fast or too slow reaction that may occur in a single curing agent. Again, from the perspective of compatibility, polyetheramine and polyamide usually have good compatibility in epoxy resin systems. This allows them to be evenly dispersed in the resin, give full play to their respective curing effects, and improve the uniformity and stability of the curing effect. Finally, the compounded curing agent can form a denser cross-linking structure, improving the resistance of the cured product to various chemical substances.

[0106] Furthermore, the epoxy adhesive component B of the present invention contains at least one of benzyl alcohol and acetophenone. Benzyl alcohol and acetophenone have a certain dissolving effect on the outermost film of the smooth floor, so that it can be used for the bonding of smooth floors with films on the surface. However, benzyl alcohol and acetophenone are flammable when exposed to open flames or high heat, which affects the flame retardant properties of the epoxy adhesive. Therefore, it is necessary to reasonably control the proportion of benzyl alcohol and acetophenone. As shown in Table 1, when the amount of modified polyether amine is reduced in the comparative example, while the proportion of components A and B remains unchanged, it is essentially equivalent to increasing the proportion of benzyl alcohol and acetophenone in component B, and the flame retardancy of the comparative example cannot meet the national standard.

[0107] The above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. An epoxy adhesive, characterized in that: It consists of separately packaged component A and component B, wherein component A consists of the following ingredients in parts by mass: 50-85 parts of epoxy resin, 3-5 parts of active diluent, 0.2-0.7 parts of coupling agent, 1.1-1.7 parts of first auxiliary agent, 10-30 parts of filler, 8-20 parts of toughening agent; The B component is composed of the following ingredients in parts by mass: 0 to 20 parts of polyamide curing agent, 0 to 55 parts of polyetheramine curing agent, 0.3 to 1.5 parts of second auxiliary agent, 15 to 72 parts of other amine curing agent, 0 to 10 parts of solvent, and 0 to 10 parts of accelerator.

2. The epoxy adhesive according to claim 1, characterized in that The mass ratio of component A to component B is 100:20-30.

3. The epoxy adhesive according to claim 1, characterized in that: The epoxy resin is at least one of bisphenol A epoxy resin, bisphenol F epoxy resin or bisphenol S epoxy resin; the active diluent is at least one of alkyl glycidyl ether, neopentyl glycol diglycidyl ether, phenyl glycidyl ether, polyphenol glycidyl ether or ethylene glycol diglycidyl ether; the coupling agent is at least one of γ-glycidyloxypropyl trimethoxysilane, γ-aminopropyl triethoxysilane or 3-glycidyloxypropyl triethoxysilane; the filler is at least one of titanium dioxide, talc, ammonium polyphosphate, aluminum hydroxide, phosphazene or mica powder; the toughening agent is carboxyl-terminated nitrile rubber, epoxy-terminated liquid nitrile rubber or hydroxyl-terminated liquid nitrile rubber.

4. The epoxy adhesive according to claim 1, characterized in that: The first auxiliary agent is at least one of a dispersant, a defoamer, a leveling agent or an antioxidant; the second auxiliary agent is at least one of a dispersant or a defoamer.

5. The epoxy adhesive according to claim 4, characterized in that: The dispersant is a high molecular polymer; the defoamer is a modified organic silicon compound; the leveling agent is a polyether modified organic silicon compound; and the antioxidant is an antioxidant.

6. The epoxy adhesive according to claim 5, characterized in that: The high molecular polymer is at least one of KYC-918, BKY-163, BYK-190, BYK-405 or KMT3331; the modified silicone compound is at least one of AKN-3801, KMT-6015, BYK-057 or BYK-088; the polyether modified silicone compound is at least one of AKN-1050, KMT-5251, KMT-5502, BYK-333 or BYK-346; the antioxidant is at least one of antioxidant 264, antioxidant 1010 or antioxidant 1076.

7. The epoxy adhesive according to claim 1, characterized in that: The polyamide curing agent is at least one of curing agents YD-8140, YD-8216, YD8200N, YD-8125A or YD-8115; the polyetheramine curing agent is at least one of polyetheramine D230, polyetheramine D400, polyetheramine D2000 or modified polyetheramine; other amine curing agents are at least one of cardanol-modified phenolic amine, N-aminoethylpiperazine, diethylenetriamine, triethylenetetramine or tetraethylenepentamine; the solvent is at least one of benzyl alcohol or acetophenone; and the accelerator is at least one of DMP-30 or 3-dimethylaminopropylamine.

8. The epoxy adhesive according to claim 7, characterized in that: The modified polyetheramine is a DEGBAE-modified polyetheramine.

9. The method for preparing the epoxy adhesive according to any one of claims 1 to 8, characterized in that: The method: Preparation of component A: Mix epoxy resin, diluent, coupling agent, first auxiliary agent and toughening agent, add filler, perform vacuum dispersion and degassing, and then pack; Preparation of component B: Mix and disperse the polyamide curing agent, polyetheramine curing agent, second auxiliary agent, other amine curing agent, solvent and accelerator in vacuum and then pack them; Preparation of epoxy adhesive: When using, mix component A and component B evenly to obtain epoxy adhesive.

10. Use of the epoxy adhesive according to any one of claims 1 to 8 in rail transit floors.

Citation Information

Patent Citations

  • Room-temperature cured epoxy resin flexible sealant and preparation method thereof

    CN102417805A

  • Dimer acid modified polyether polyamine compound as well as preparation method and application thereof

    CN112457190A

  • Normal-temperature curing epoxy resin-based vitrimer adhesive and preparation method thereof

    CN113337234A

  • Conductive epoxy adhesive for bonding floor cloth and preparation method of conductive epoxy adhesive

    CN115141589A