High-stability heat transfer medium and preparation method thereof

By using water, alcohols, pyrrolidone carboxylate, modified nanotitanium dioxide, antioxidants and stabilizers in the heat transfer medium, combined with activated nanotitanium dioxide and ultrasonic treatment, the poor stability of the heat transfer medium at high temperatures is solved. The problem is that efficient heat transfer performance and long-term stability are achieved.

CN118931503APending Publication Date: 2024-11-12HAINAN DEHAI ZHIYUAN INVESTMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410980985.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing heat transfer medium has poor stability and reduced heat transfer efficiency under high temperature or long-term operating conditions, which affects the normal operation of the equipment and may lead to energy waste and safety hazards.

Method used

Using a combination of water, alcohols, pyrrolidone carboxylate, modified nanotitanium dioxide, antioxidants and stabilizers, nanotitanium dioxide is activated by citric acid and sodium selenite, combined with ultrasonic treatment and stirring reaction, a high stability transmission is prepared. Thermal medium ensures that the modified nanotitanium dioxide continuously outputs free radicals to improve the stability of the medium.

Benefits of technology

It achieves high heat transfer efficiency and stability under high temperature or long-term operating conditions, effectively solves the problems of reduced heat transfer efficiency and poor stability, and improves the overall performance of the medium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956057700000031
    Figure BDA0004956057700000031
  • Figure BDA0004956057700000041
    Figure BDA0004956057700000041
  • Figure BDA0004956057700000061
    Figure BDA0004956057700000061
Patent Text Reader

Abstract

The invention relates to the technical field of heat transfer media, and particularly discloses a high-stability heat transfer medium and a preparation method thereof. The invention discloses a high-stability heat transfer medium. The high-stability heat transfer medium is prepared from the following components in parts by weight: 100-140 parts of water, 50-60 parts of alcohol substances, 10-20 parts of pyrrolidone carboxylate, 5-10 parts of modified nano titanium dioxide, 1-5 parts of an antioxidant and 2-6 parts of a stabilizer, the antioxidant is formed by mixing 2, 6-butylated hydroxytoluene and D-sodium erythorbate according to the weight ratio of (1 to 3): (1 to 3); the stabilizer is formed by mixing pyrrolidone carboxylate and organic phosphoric acid substances according to the weight ratio of (1-5): (5-9). Through reasonable component selection and proportioning and combination with an optimized preparation method, the prepared heat transfer medium not only has excellent heat transfer efficiency, but also can keep excellent stability under the condition of high temperature or long-term operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of heat transfer media, and in particular to a high-stability heat transfer medium and a preparation method thereof. Background Art

[0002] Heat transfer media are widely used in industrial production, energy conversion, electronic equipment and other fields. As a part of thermal energy engineering, heat transfer media generally need to enter the interlayer of the reactor to achieve cooling or heating of the reactor through heat exchange.

[0003] However, existing heat transfer media often have problems such as poor stability and reduced heat transfer efficiency under high temperature or long-term operation conditions. These problems not only affect the normal operation of the equipment, but may also lead to energy waste and safety hazards. Therefore, developing a heat transfer medium with high stability to improve heat transfer efficiency and equipment reliability has become an urgent problem to be solved. Summary of the invention

[0004] In order to solve the technical problems that the existing heat transfer medium has poor stability and reduced heat transfer efficiency under high temperature or long-term operation conditions, the present application provides a high-stability heat transfer medium and a preparation method thereof.

[0005] The present application provides a high-stability heat transfer medium, which specifically includes the following components in parts by weight: 100-140 parts of water, 50-60 parts of alcohol substances, 10-20 parts of pyrrolidone carboxylate, 5-10 parts of modified nano titanium dioxide (nano aluminum oxide), 1-5 parts of antioxidants, and 2-6 parts of stabilizers; The modified nano titanium dioxide is prepared by the following preparation method: adding nano titanium dioxide to a 20-30wt% ethanol aqueous solution at a temperature of 60-80°C, ultrasonically treating for 20-40 minutes, then adding citric acid and sodium selenite, stirring and reacting for 90-120 minutes, centrifugally filtering, and drying to obtain the modified nano titanium dioxide; the weight ratio of the nano titanium dioxide, citric acid, and sodium selenite is 20-25:10-15:0.5-1.5; The antioxidant is composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1-3:1-3; The stabilizer is composed of a mixture of pyrrolidone carboxylate and organic phosphoric acid substances in a weight ratio of 1-5:5-9.

[0006] The present application successfully develops a high-stability heat transfer medium through reasonable component selection and ratio; the heat transfer medium not only has excellent heat transfer efficiency, but also can maintain excellent stability under high temperature or long-term operation conditions, effectively solving the problems of decreased heat transfer efficiency and poor stability in the prior art.

[0007] This application uses citric acid and sodium selenite to activate nano titanium dioxide, so that the heat transfer medium can play a certain role in the use of the heat transfer medium, stimulate the modified nano titanium dioxide to produce strong oxidizing free radicals, thereby inactivating the hydroxyl groups of active alcohol substances, and effectively improving the stability of the heat transfer medium. At the same time, this application uses a weight ratio of 1-3:1-3 of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate to form an antioxidant, and a weight ratio of 1-5:5-9 of pyrrolidone carboxylate and organic phosphoric acid to form a stabilizer, and reasonably selects components and ratios. On the basis of ensuring the continuous output of free radicals of the modified nano titanium dioxide, it further synergizes with other raw material components to effectively further improve the stability of the heat transfer medium.

[0008] Preferably, the high-stability heat transfer medium specifically comprises the following components in parts by weight: 110-130 parts of water, 53-57 parts of alcohol substances, 13-17 parts of pyrrolidone carboxylate, 6-9 parts of modified nano titanium dioxide, 2-4 parts of antioxidants, and 3-5 parts of stabilizers.

[0009] Preferably, in the preparation method of the modified nano-titanium dioxide, the weight ratio of the nano-titanium dioxide, citric acid and sodium selenite is 21-24:12-14:0.8-1.2.

[0010] Preferably, the antioxidant is composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1-2:2-3.

[0011] Through experimental analysis, it can be known that the present application selects the above-mentioned weight ratio of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate to mix and form an antioxidant, which can effectively improve the stability of the heat transfer medium.

[0012] Preferably, the stabilizer is composed of a mixture of pyrrolidone carboxylate and organic phosphoric acid substances in a weight ratio of 2-4:6-8.

[0013] Through experimental analysis, it can be known that the present application selects the above-mentioned weight ratio of pyrrolidone carboxylate and organic phosphoric acid substances to mix and form a stabilizer, which can effectively improve the stability of the heat transfer medium.

[0014] Preferably, the organic phosphoric acid substance is selected from one or more of diethylenetriamine pentamethylene sodium phosphate, ethylenediaminetetramethylene phosphate, and aminotrimethylene phosphate.

[0015] Preferably, the alcohol substance is composed of a mixture of mannitol and polyethylene glycol in a weight ratio of 10:1-10.

[0016] Preferably, the alcohol substance is composed of a mixture of mannitol and polyethylene glycol in a weight ratio of 10:1-4.

[0017] Preferably, the pyrrolidone carboxylate is selected from one or more of sodium pyrrolidone carboxylate, potassium pyrrolidone carboxylate, zinc pyrrolidone carboxylate, copper pyrrolidone carboxylate and calcium pyrrolidone carboxylate.

[0018] In a second aspect, the present application provides a method for preparing the above-mentioned high-stability heat transfer medium, which specifically comprises the following steps: adding pyrrolidone carboxylate, an antioxidant, and a stabilizer to water under normal pressure and a temperature of 40-60° C., and stirring for 20-30 minutes; Add the modified nano titanium dioxide and perform ultrasonic treatment for 30-50 minutes; The alcohol substance is added, stirred for 5-10 minutes, and cooled to room temperature to obtain the high-stability heat transfer medium.

[0019] In summary, the technical solution of this application has the following effects: The present application successfully developed a high-stability heat transfer medium through reasonable component selection and ratio, combined with an optimized preparation method. The heat transfer medium not only has excellent heat transfer efficiency, but also maintains excellent stability under high temperature or long-term operation conditions, effectively solving the problems of reduced heat transfer efficiency and poor stability in the prior art.

[0020] The present application further improves the stability of the heat transfer medium while ensuring that the heat transfer medium has a high thermal conductivity by specifically selecting the types and amounts of antioxidants and stabilizers. DETAILED DESCRIPTION

[0021] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application. Example

[0022] Examples 1-5 Examples 1-5 each provide a high stability heat transfer medium.

[0023] The difference between the above embodiments is that the dosage of each component in the high stability heat transfer medium is different, as shown in Table 1.

[0024] The preparation method of the heat transfer medium in the above embodiment is: The modified nano titanium dioxide is prepared by the following method: 23 g of nano titanium dioxide (average particle size of 5-50 nm) is added to 100 g of 25 wt% ethanol aqueous solution at 70° C., ultrasonic treatment is performed at 200 W for 30 min, and then 13 g of citric acid and 1 g of sodium selenite are added, stirring and reacting is continued for 100 min, centrifugation is performed, and vacuum drying is performed at 80° C. to obtain the modified nano titanium dioxide; Under normal pressure and temperature of 5°C, zinc pyrrolidone carboxylate, an antioxidant (composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1:2), and a stabilizer (composed of pyrrolidone carboxylate and ethylenediaminetetramethylene phosphate in a weight ratio of 3:7) were added to water and stirred for 25 minutes; Add modified nano-titanium dioxide and treat with ultrasound for 40 min; An alcohol substance (composed of a mixture of mannitol and polyethylene glycol in a weight ratio of 10:2) was added, stirred for 8 minutes, and cooled to room temperature to obtain a heat transfer medium.

[0025] Table 1 Amount of each component in the high stability heat transfer medium in Examples 1-5 and Comparative Example 1 Embodiment 6-9 Examples 6-9 each provide a high stability heat transfer medium.

[0026] The difference between the above embodiment and embodiment 2 is that the preparation method of modified nano titanium dioxide is different, as shown below.

[0027] In Example 6: modified nano titanium dioxide is obtained by the following preparation method: at a temperature of 70°C, 20g of nano titanium dioxide (average particle size of 5-50nm) is added to 100g of a 25wt% ethanol aqueous solution, and ultrasonic treatment is performed at a power of 200w for 30min, and then 15g of citric acid and 0.5g of sodium selenite are added, and the reaction is continued to stir for 100min, centrifuged and dried in vacuo at 80°C to obtain modified nano titanium dioxide.

[0028] In Example 7: The modified nano titanium dioxide was prepared by the following method: 25 g of nano titanium dioxide (average particle size of 5-50 nm) was added to 100 g of a 25 wt% ethanol aqueous solution at 70°C, and ultrasonic treatment was performed at 200 W for 30 min, followed by addition of 10 g of citric acid and 1.5 g of sodium selenite, and the reaction was continued with stirring for 100 min, centrifuged and dried in vacuo at 80°C to obtain the modified nano titanium dioxide.

[0029] In Example 8: Modified nano titanium dioxide is obtained by the following preparation method: 23g of nano titanium dioxide (average particle size of 5-50nm) is added to 100g of 20wt% ethanol aqueous solution at a temperature of 60°C, and ultrasonic treatment is performed at a power of 200w for 30min, and then 13g of citric acid and 1g of sodium selenite are added, and the reaction is continued to stir for 100min, centrifugally filtered, and vacuum dried at 80°C to obtain modified nano titanium dioxide.

[0030] In Example 9: Modified nano titanium dioxide is obtained by the following preparation method: 23g of nano titanium dioxide (average particle size of 5-50nm) is added to 100g of 25wt% ethanol aqueous solution at a temperature of 80°C, and ultrasonic treatment is performed at a power of 200w for 30min, and then 13g of citric acid and 1g of sodium selenite are added, and the reaction is continued to stir for 100min, centrifugally filtered, and vacuum dried at 80°C to obtain modified nano titanium dioxide.

[0031] The other raw materials and their amounts and the preparation method of the high-stability heat transfer medium in the above embodiment are the same as those in Example 2.

[0032] Examples 10-13 Examples 10-13 each provide a high stability heat transfer medium.

[0033] The difference between the above embodiment and embodiment 2 is that the types of antioxidants are different, as shown below.

[0034] In Example 10, the antioxidant is composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 3:2.

[0035] In Example 11, the antioxidant is composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 2:1.

[0036] In Example 12, the antioxidant is composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1:3.

[0037] In Example 13: the antioxidant is composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 2:2 (1:1).

[0038] The other raw materials and their amounts and the preparation method of the high-stability heat transfer medium in the above embodiment are the same as those in Example 2.

[0039] Examples 14-17 Examples 14-17 each provide a high stability heat transfer medium.

[0040] The difference between the above embodiment and embodiment 2 is that the types of stabilizers are different, as shown below.

[0041] In Example 14: the stabilizer is composed of a mixture of zinc pyrrolidone carboxylate and ethylenediaminetetramethylene phosphate in a weight ratio of 1:5.

[0042] In Example 15, the stabilizer is composed of a mixture of zinc pyrrolidone carboxylate and ethylenediaminetetramethylene phosphate in a weight ratio of 5:9.

[0043] In Example 16: the stabilizer is composed of a mixture of potassium pyrrolidonecarboxylate and ethylenediaminetetramethylene phosphate in a weight ratio of 3:7.

[0044] In Example 17: the stabilizer is composed of a mixture of calcium pyrrolidonecarboxylate and ethylenediaminetetramethylene phosphate in a weight ratio of 3:7.

[0045] The other raw materials and their amounts and the preparation method of the high-stability heat transfer medium in the above embodiment are the same as those in Example 2.

[0046] Comparative Example Comparative Example 1 This comparative example provides a heat transfer medium.

[0047] The difference between this comparative example and Example 2 is that the dosage of each raw material component is different, as shown in Table 1.

[0048] The other raw materials and their amounts and the preparation method of the high-stability heat transfer medium in this comparative example are the same as those in Example 2.

[0049] Comparative Examples 2-4 Comparative Examples 2-4 each provide a heat transfer medium.

[0050] The differences between the above comparative example and Example 2 are specifically as follows.

[0051] In Comparative Example 2: an equal amount of unmodified nano-titanium dioxide is used to replace the modified nano-titanium dioxide.

[0052] In Comparative Example 3: an equal amount of modified nano-alumina was used instead of modified nano-titanium dioxide; the modified nano-alumina was prepared by the following method: 23 g of nano-alumina (average particle size of 5-50 nm) was added to 100 g of 25 wt% ethanol aqueous solution at a temperature of 70°C, and ultrasonic treatment was performed at a power of 200 W for 30 min, and then 13 g of citric acid and 1 g of sodium sulfite were added, and the reaction was continued with stirring for 100 min, centrifuged and dried in vacuo at 80°C to obtain modified nano-alumina.

[0053] In Comparative Example 4, the antioxidant is composed of a mixture of 4,4-methylenebis-2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1:2.

[0054] The other raw materials and their amounts and the preparation method of the high-stability heat transfer medium in the above comparative example are the same as those in Example 2.

[0055] Comparative Example 5 This comparative example provides a heat transfer medium with high stability.

[0056] The difference between this comparative example and Example 2 is that no stabilizer is added.

[0057] The preparation method of the heat transfer medium in this comparative example is: The modified nano titanium dioxide is prepared by the following method: 23 g of nano titanium dioxide (average particle size of 5-50 nm) is added to 100 g of 25 wt% ethanol aqueous solution at 70° C., ultrasonic treatment is performed at 200 W for 30 min, and then 13 g of citric acid and 1 g of sodium selenite are added, stirring and reacting is continued for 100 min, centrifugation is performed, and vacuum drying is performed at 80° C. to obtain the modified nano titanium dioxide; Under normal pressure and temperature of 5°C, zinc pyrrolidone carboxylate and an antioxidant (composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1:2) were added to water and stirred for 25 minutes; Add modified nano-titanium dioxide and treat with ultrasound for 40 min; An alcohol substance (composed of a mixture of mannitol and polyethylene glycol in a weight ratio of 10:2) was added, stirred for 8 minutes, and cooled to room temperature to obtain a heat transfer medium.

[0058] Performance test thermal conductivity: The thermal conductivity of the heat transfer medium in the embodiment and the comparative example (under different temperature conditions: 20°C, 60°C, 100°C) was tested; High temperature stability test: The heat transfer medium in the embodiment and the comparative example is placed at a test temperature of 20°C for 1200 hours; a test temperature of 60°C for 1200 hours; and a test temperature of 100°C for 1200 hours. The thermal conductivity performance of the heat transfer medium is tested to evaluate the high temperature stability, high temperature stability = thermal conductivity of the sample after the high temperature stability test / thermal conductivity of the original sample before the test × 100%.

[0059] Corrosion inhibition performance test: The static hanging piece weight loss method was used to evaluate the corrosion of the heat transfer medium to Q235 steel; the test time was 1200 hours and the test temperature was 50°C.

[0060] Test results: as shown in Table 2.

[0061] Table 2 Performance test results of heat transfer medium in Examples 1-17 and Comparative Examples 1-5 Combined with Table 2, by comparing the test results of the embodiment and the comparative example, it can be seen that the present application successfully developed a high-stability heat transfer medium through reasonable component selection and ratio, combined with an optimized preparation method. The heat transfer medium not only has excellent heat transfer efficiency, but also can maintain excellent stability under high temperature or long-term operation conditions, effectively solving the problems of reduced heat transfer efficiency and poor stability in the prior art.

[0062] By comparing the test results of Examples 1-5 with those of Comparative Example 1, it can be seen that the present application reasonably proportions the amounts of the various raw material components so that the heat transfer medium prepared has higher stability.

[0063] By comparing the test results of Examples 2, 6-9 with Comparative Examples 2-3, it can be seen that in Comparative Example 2, an equal amount of unmodified nano-titanium dioxide is used to replace the modified nano-titanium dioxide, and the thermal conductivity of the heat transfer medium prepared is low and the stability is poor; in Comparative Example 3, an equal amount of modified nano-aluminum oxide is used to replace the modified nano-titanium dioxide, and the stability of the heat transfer medium prepared is poor; and the heat transfer medium prepared by using modified nano-titanium dioxide in the present application has higher stability.

[0064] By comparing the test results of Examples 2, 10-13 with Comparative Example 4, it can be seen that the present application uses a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1-3:1-3 to form an antioxidant, which further improves the stability of the heat transfer medium.

[0065] By comparing the test results of Examples 2, 14-17 with Comparative Example 5, it can be seen that the present application uses a mixture of pyrrolidone carboxylate and organic phosphoric acid substances in a weight ratio of 1-5:5-9 to form a stabilizer, which further improves the stability of the heat transfer medium.

[0066] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A high stability heat transfer medium, characterized in that: Specifically, it includes the following components in parts by weight: 100-140 parts of water, 50-60 parts of alcohol substances, 10-20 parts of pyrrolidone carboxylate, 5-10 parts of modified nano titanium dioxide (nano aluminum oxide), 1-5 parts of antioxidants, and 2-6 parts of stabilizers; The modified nano titanium dioxide is prepared by the following preparation method: adding nano titanium dioxide to a 20-30wt% ethanol aqueous solution at a temperature of 60-80°C, ultrasonically treating for 20-40 minutes, then adding citric acid and sodium selenite, stirring and reacting for 90-120 minutes, centrifugally filtering, and drying to obtain the modified nano titanium dioxide; the weight ratio of the nano titanium dioxide, citric acid, and sodium selenite is 20-25:10-15:0.5-1.5; The antioxidant is composed of a mixture of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate in a weight ratio of 1-3:1-3; The stabilizer is composed of a mixture of pyrrolidone carboxylate and organic phosphoric acid substances in a weight ratio of 1-5:5-9.

2. The high stability heat transfer medium according to claim 1, characterized in that: The high-stability heat transfer medium specifically comprises the following components in parts by weight: 110-130 parts of water, 53-57 parts of alcohol substances, 13-17 parts of pyrrolidone carboxylate, 6-9 parts of modified nano titanium dioxide, 2-4 parts of antioxidants, and 3-5 parts of stabilizers.

3. The high stability heat transfer medium according to claim 1, characterized in that: In the preparation method of the modified nano titanium dioxide, the weight ratio of the nano titanium dioxide, citric acid and sodium selenite is 21-24:12-14:0.8-1.

2.

4. The high stability heat transfer medium according to claim 1, characterized in that: The antioxidant is composed of 2,6-di-tert-butyl-p-cresol and sodium D-isoascorbate mixed in a weight ratio of 1-2:2-3.

5. The high stability heat transfer medium according to claim 1, characterized in that: The stabilizer is composed of a mixture of pyrrolidone carboxylate and organic phosphoric acid substances in a weight ratio of 2-4:6-8.

6. The high stability heat transfer medium according to claim 1, characterized in that: The organic phosphoric acid substance is selected from one or more of diethylenetriamine pentamethylene sodium phosphate, ethylenediaminetetramethylene phosphate, and aminotrimethylene phosphate.

7. The high stability heat transfer medium according to claim 1, characterized in that: The alcohol substance is composed of a mixture of mannitol and polyethylene glycol in a weight ratio of 10:1-10.

8. The high stability heat transfer medium according to claim 7, characterized in that: The alcohol substance is composed of a mixture of mannitol and polyethylene glycol in a weight ratio of 10:1-4.

9. The high stability heat transfer medium according to claim 1, characterized in that: The pyrrolidone carboxylate is selected from one or more of sodium pyrrolidone carboxylate, potassium pyrrolidone carboxylate, zinc pyrrolidone carboxylate, copper pyrrolidone carboxylate and calcium pyrrolidone carboxylate.

10. The method for preparing a high-stability heat transfer medium according to any one of claims 1 to 9, characterized in that: The specific steps include: Under normal pressure and temperature of 40-60°C, add pyrrolidone carboxylate, antioxidant and stabilizer into water and stir for 20-30 minutes; Add the modified nano titanium dioxide and perform ultrasonic treatment for 30-50 minutes; The alcohol substance is added, stirred for 5-10 minutes, and cooled to room temperature to obtain the high-stability heat transfer medium.