Process for extracting copper element from residual silicon powder of polycrystalline silicon and organic silicon

By dissolving and distilling ammonia treatment with ammonia water and ammonium salt solution, combined with solid-liquid separation and oxygen plasma treatment, the problem of difficult dissolution of copper catalysts is solved, the recycling efficiency and resource utilization of copper elements are improved, and the wastewater emission is achieved.

CN118932178APending Publication Date: 2024-11-12NINGXIA SHENGLAN CHEM ENVIRONMENTAL PROT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983143.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, copper catalysts are difficult to completely dissolve, resulting in problems such as copper metal residues, waste of resources and reduced treatment efficiency.

Method used

The copper waste contacts are dissolved by a mixed solution of ammonia water and ammonium salt. The copper-containing precipitate is obtained by distilling ammonia, and silver oxide is obtained by sintering. Combined with solid-liquid separation and oxygen plasma treatment, the dissolution and recovery efficiency of copper is improved.

Benefits of technology

This reduces the residual problem of copper metal, improves the recycling efficiency of copper elements, achieves zero wastewater discharge, and makes the recovered silicon powder available for ingot formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932178A_ABST
    Figure CN118932178A_ABST
Patent Text Reader

Abstract

The invention relates to a process method for extracting a copper element from residual silicon powder of polycrystalline silicon and organic silicon, which is characterized by comprising the following steps of: dissolving a copper waste contact body by using a mixed solution of ammonia water and ammonium salt, collecting and recovering the solution, carrying out ammonia distillation treatment to obtain a copper-containing precipitate, and sintering the copper-containing precipitate to obtain copper oxide. And the problem of copper metal residues in the treatment process is solved, waste in copper element recovery is reduced, and the treatment efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental protection, and in particular relates to a process for extracting copper elements from polysilicon and residual silicon powder of organic silicon. Background Art

[0002] Silicone and polysilicon are important basic materials in modern industry and science and technology. Due to their unique chemical and physical properties, silicone materials are used as ideal sealing materials, protective or insulating coatings in the fields of aerospace, electronics and construction. In the chemical industry, silicone can also be used to produce chemical raw materials such as coupling agents, silicone resins, silicone oils and silicone rubbers. Polysilicon is an important material in semiconductor devices and the photovoltaic industry. The production of silicone and polysilicon is an important link in the industrial manufacturing chain. With the continuous advancement of the production technology of silicone and polysilicon, the production scale of silicone and polysilicon is getting larger and larger. At the same time, the environmental impact of the production process of silicone and polysilicon has gradually attracted attention.

[0003] Copper catalysts are used in the production of organosilicon and polysilicon. Ternary copper catalysts are usually used in organosilicon production, and cuprous chloride catalysts are usually used in polysilicon production. Unreacted silicon powder is produced in the polysilicon cold hydrogenation reactor and the organosilicon synthesis reactor. This part of silicon powder is enriched with deactivated copper catalysts. The copper content of the unreacted silicon powder produced by polysilicon cold hydrogenation is about 2-3%, and the silicon powder has the risk of spontaneous combustion and the production of volatile hydrogen chloride. The copper content of the unreacted silicon powder produced by the organosilicon synthesis furnace is about 4-10%. The silicon powder is highly active and prone to spontaneous combustion.

[0004] In the prior art, such as Chinese patent CN113699378B, an acid leaching process and an iron powder reduction process are used to recover the copper element in the Cu catalyst in the residual silicon powder. However, the process has a low copper recovery rate, produces a large amount of strongly acidic ferric chloride wastewater, and copper ions remain in the wastewater. The wastewater is a hazardous waste containing heavy metals, and the on-site environment is harsh. In addition, in the prior art, such as CN102795653A, an ammonia method is used to treat the Cu catalyst, and the copper in the waste contact body is leached by an ammonia water-ammonium salt solution to form a soluble complex. Then, high-purity copper oxide is separated and recovered by an ammonia evaporation process. This process avoids the environmental problems of the traditional acid leaching method, simplifies the process, reduces costs, and improves the recovery efficiency of metals. However, the process currently still has the following problems: the copper catalyst is difficult to completely dissolve, and the residual copper metal means a waste of resources and a reduction in processing efficiency.

[0005] Therefore, it is necessary to provide a process for extracting copper from polycrystalline silicon and residual silicon powder of organic silicon. This method can reduce the problem of residual copper metal during the treatment process, reduce the waste in copper recovery, and improve the treatment efficiency. The silicon powder after copper recovery can be directly used for casting to form silicon ingots, and at the same time, zero wastewater discharge is achieved in the whole process. Summary of the invention

[0006] The technical problem to be solved by the present invention is that the copper catalyst is difficult to completely dissolve, and the residual copper metal causes waste of resources and reduced processing efficiency. Therefore, it is necessary to provide a process for extracting copper from polysilicon and organic silicon residual silicon powder to solve the above problem.

[0007] The technical solution adopted by the present invention to solve the technical problem is:

[0008] The invention discloses a process for extracting copper from polysilicon and residual silicon powder of organic silicon, characterized in that the process comprises: using a mixed solution of ammonia water and ammonium salt to dissolve the copper waste contact body, collecting and recovering the solution, and performing ammonia evaporation treatment to obtain a copper-containing precipitate, and sintering the copper-containing precipitate to obtain copper oxide.

[0009] Specifically, the ammonium salt is at least one of Cl-, OH-, CO32-, and HCO3- salts of NH4+.

[0010] Specifically, the copper-containing precipitate is a solid mixture of one or more of cupric chloride, cuprous chloride, cupric oxide, cuprous oxide, cupric hydroxide, cuprous hydroxide, and basic copper carbonate.

[0011] Specifically, before using the mixed solution of ammonia water and ammonium salt to dissolve the copper waste contacts, a solid-liquid separation step is also included.

[0012] Specifically, the object of solid-liquid separation is a mixture of silicon powder and chlorosilane.

[0013] Specifically, the solid-liquid separation uses a centrifugal drying device.

[0014] Specifically, the content of chlorosilane in the silicon powder is controlled within 10% by solid-liquid separation.

[0015] Specifically, the content of chlorosilane in the silicon powder is controlled within 1% by solid-liquid separation.

[0016] Specifically, the process parameters of the centrifugal drying equipment include: a rotation speed of 800-1000 rpm, an operating pressure controlled at 5-150 Kpa, and an operating temperature controlled at 5-300°C.

[0017] Specifically, ammonia evaporation also produces ammonia gas.

[0018] The present invention has the following beneficial effects:

[0019] 1) Provided is a process for extracting copper from polysilicon and residual silicon powder of organic silicon. The method can reduce the problem of residual copper metal during the treatment process, reduce the waste in copper recovery, and improve the treatment efficiency. The silicon powder after copper recovery can be directly used for casting to form silicon ingots, and at the same time, zero wastewater discharge is achieved in the whole process.

[0020] 2) The remaining solid waste contact body is subjected to plasma treatment. Oxygen plasma treatment increases the surface energy of the particles, improves wettability and adhesion, and the silicon particles treated with oxygen plasma usually show enhanced hydrophilicity, which is beneficial for further reactions in subsequent aqueous dispersions. In addition, after the copper-containing material is treated with oxygen plasma, more copper is oxidized to copper oxide. Since copper oxide is an alkaline oxide, it is easier to react with NH4 + (ammonium ions) react with NH3 (ammonia gas) and then dissolve in the treatment solution to achieve full dissolution of copper. It has certain chemical activity and can react with acidic or alkaline substances under appropriate conditions.

[0021] 3) In the secondary dissolution treatment, the ammonia content of the ammonia-ammonium salt mixture is higher than that of the first dissolution treatment. Compared with the first dissolution treatment, the copper compound in the secondary dissolution treatment is closer to the core of the material, with a denser texture and more complex compound conditions. Therefore, compared with the first dissolution treatment, the treatment liquid of the secondary dissolution treatment needs to have stronger copper dissolution properties. However, the ammonia content in the secondary dissolution treatment cannot be too large, for example, greater than the molar ratio of ammonia to ammonium salt of 5:1. Since the secondary treatment liquid after the secondary dissolution needs to be treated with ammonia evaporation precipitation, excessive NH3 content will cause the overall acid-base imbalance of the recovered solution, which tends to be alkaline, which is not conducive to the precipitation of precipitation.

[0022] 4) A proper amount of ammonium salt is added in the ammonia evaporation step to adjust the acidity and alkalinity of the recovered solution, thereby making the solution acidic during the ammonia evaporation process, which is conducive to the precipitation of copper precipitation.

[0023] 5) Rationally adjust various process parameters to synergistically optimize process effects and extraction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to clearly illustrate the technical solution of the present invention, the drawings of specific implementation methods are briefly introduced below.

[0025] Figure 1 The process of extracting copper from residual silicon powder provided by the present invention

[0026] Figure 2 XRD spectrum of copper oxide extracted by the present invention DETAILED DESCRIPTION

[0027] The present invention will be described in more detail below with reference to the accompanying drawings, in which preferred embodiments of the present invention are shown, and it should be understood that those skilled in the art can modify the present invention described herein and still achieve the beneficial effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art, and not as a limitation of the present invention.

[0028] For the sake of clarity, not all features of the actual embodiments are described. In the following description, well-known functions and structures are not described in detail because they would obscure the present invention with unnecessary details. It should be recognized that in the development of any actual embodiment, a large number of implementation details must be made to achieve the specific goals of the developer.

[0029] In order to make the purpose and features of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the accompanying drawings are all in a very simplified form and use non-precise ratios, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0030] The present invention provides a process for extracting copper from polysilicon and residual silicon powder of organic silicon, see the attached Figure 1 The process flow includes: 1) subjecting a mixture of silicon powder and chlorosilane to a centrifugal and drying process to obtain a copper waste contact (a solid mixture of silicon powder, copper, and copper oxide); 2) mixing the above copper waste contact with an ammonia-ammonium salt mixed solution for a first dissolution treatment, and obtaining a first recovery solution and remaining solid waste contacts through the first dissolution treatment; 3) subjecting the remaining solid waste contacts to an oxygen plasma treatment to obtain a solid waste contact with a surface oxidation treatment; 4) dispersing the solid waste contact with a surface oxidation treatment in a solvent and subjecting it to a secondary dissolution treatment to obtain silicon powder (which can be subsequently recovered and used for casting to form silicon ingots) and a second recovery solution; 5) collecting the first and second recovery solutions and subjecting them to ammonia evaporation to obtain copper precipitate and ammonia gas (which can be recovered and dissolved in ammonia water as a reaction raw material), wherein the copper precipitate can be further subjected to a sintering reaction to obtain copper oxide (as a new catalyst).

[0031] Specifically, the specific processes of the above steps are as follows:

[0032] 1) The mixture of silicon powder and chlorosilane is first subjected to centrifugation and drying processes to obtain a copper waste contact (a solid mixture of silicon powder, copper and copper oxide), including:

[0033] The mixture containing silicon powder and chlorosilane enters a liquid-solid separation device (preferably a centrifugal drying device), and the content of chlorosilane in the silicon powder is controlled within 10% by solid-liquid separation, preferably within 1%. Drying equipment and processes are common knowledge in the field, and those skilled in the art can reasonably select solid-liquid separation equipment and corresponding process parameters based on the existing technology. As an example, a centrifugal drying device can be selected with a rotation speed of 800-1000 rpm, an operating pressure controlled at 5-150Kpa, and an operating temperature controlled at 5-300°C to separate silicon powder from chlorosilane to obtain a copper waste contact solid, which includes: a solid mixture and / or composite of silicon powder, copper, and copper oxide.

[0034] 2) Mixing the copper waste contacts and the ammonia-ammonium salt mixed solution for a first dissolution treatment, and obtaining a first recovery solution and remaining solid waste contacts through the first dissolution treatment, including:

[0035] The solid copper waste contact body is placed into a container, and an ammonia-ammonium salt mixed solution is added to the container, the ammonium salt is (NH4)2CO3, the ammonium salt solution concentration is 30wt%, the molar ratio of ammonia to ammonium salt in the ammonia-ammonium salt mixed solution is 2:1, and the mass ratio of the ammonia-ammonium salt mixed solution to the copper waste contact body is 1:1. The container is closed and sealed, and oxygen is introduced into the container through an oxygen ventilation pipe until the pressure in the container reaches 2-3 atmospheres, preferably 2 atmospheres. The reaction temperature is 80 degrees Celsius, and the reaction time is 8-10 hours, preferably 10 hours.

[0036] Since there are multiple valence states of copper in the copper waste contact, namely Cu, Cu+, and Cu2+, and the conversion of Cu and Cu+ requires sufficient oxygen to participate in the reaction. Therefore, a certain pressure of oxygen is injected into the sealed reaction vessel, and the copper in the copper waste contact can be more effectively oxidized under pressurized conditions. In an aerobic environment, copper can be oxidized into copper ions. In addition, increasing the pressure can increase the solubility of the gas, so the solubility of oxygen in the solution is higher under high pressure, which means that more oxygen molecules can participate in the reaction, thereby accelerating the rate of the oxidation reaction. Pressurized oxygen also helps to ensure that the copper in the copper waste contact is completely oxidized, improving the recovery rate and conversion rate of copper. Under higher oxygen partial pressures, even if the copper waste contact contains copper forms that are difficult to oxidize, it can be fully oxidized. The presence of oxygen can also inhibit unwanted side reactions, such as preventing the reduction of other metals or impurities, and ensuring the selective extraction of copper.

[0037] Preferably, during the first dissolution treatment, a stirrer or ultrasonic vibration may be used to promote the complete dissolution of copper in the waste contact body.

[0038] After the first dissolution treatment, a first recovery solution and the remaining solid waste contacts are obtained. The first recovery solution dissolves copper from a portion of the waste contacts, and a portion of copper from the remaining solid waste contacts remains on or between the solid silicon powders.

[0039] 3) treating the remaining solid waste contacts with oxygen plasma to obtain solid waste contacts with surface oxidation treatment, including:

[0040] The remaining solid waste contacts are transferred to a plasma treatment chamber and subjected to plasma treatment. The oxygen plasma treatment increases the surface energy of the particles, improves wettability and adhesion, and the silicon particles treated with oxygen plasma generally show enhanced hydrophilicity, which is beneficial for further reactions in subsequent aqueous dispersions.

[0041] During oxygen plasma treatment, the waste contacts can be dispersed and layered on a carrier, or layered using a multi-layered device, thereby increasing the contact area with the plasma.

[0042] In addition, after the copper-containing material is treated with oxygen plasma, more copper is oxidized to copper oxide. Since copper oxide is an alkaline oxide, it is easier to react with NH4 + (ammonium ions) react with NH3 (ammonia gas) and then dissolve in the treatment solution to achieve full dissolution of copper. It has certain chemical activity and can react with acidic or alkaline substances under appropriate conditions.

[0043] Specific processing parameters include: introducing argon and oxygen (molar ratio 3:2) into the plasma processing chamber, vacuum pressure 75Pa-90Pa, bias 600-800V, power 1.5-2KW, temperature 150-180 degrees Celsius, processing time = 20 minutes + 35 seconds * N, where N = (M-600g) / 100g, that is, N is based on 600g, and 1 is counted for every 100g increase in mass.

[0044] Regarding the treatment parameters, it should be pointed out that: since oxygen plasma treatment mainly achieves two effects: further oxidation of copper and improvement of the hydrophilicity and dispersibility of the particles. The above two effects are very sensitive to the process. Through orthogonal experiments, it can be obtained that: when the molar ratio of argon and oxygen is greater than 3:2 or the temperature is too low, the oxidation of copper is insufficient, which reduces the final copper recovery rate; and when the molar ratio of argon and oxygen is less than 3:2 or the temperature is too high, the silicon oxide formed on the silicon surface is too thick, resulting in reduced dispersibility of silicon particles. When the bias or power is too small, the plasma energy is too low, which is not conducive to surface treatment. When the bias or power is too small, the plasma energy is too high, which will cause the concave-convex structure on the particle surface to be too large, resulting in hydrophobicity. In addition, too long or too short a treatment time also causes a large deviation in the degree of copper oxidation. Therefore, the above plasma treatment parameters synergistically achieve a higher Cu oxidation effect and a moderate particle surface state.

[0045] 4) dispersing the remaining solid waste contact after the surface oxidation treatment in a solvent, and performing a secondary dissolution treatment to obtain silicon powder (which can be subsequently recovered and used for ingot casting to form a silicon ingot) and a second recovery solution; dispersing in a solvent, and performing a secondary dissolution treatment to obtain silicon powder (which can be subsequently recovered and used for ingot casting to form a silicon ingot) and a second recovery solution, comprising:

[0046] The remaining solid waste contact body after oxygen plasma treatment is transferred to a solid-liquid reaction container, and a solvent is added, and the solvent can be deionized water. The mass ratio of the solvent to the remaining solid waste contact body is 10-15:1, preferably 10:1, and an ammonia-ammonium salt mixed solution is added to the container, the ammonium salt is (NH4)2CO3, the ammonium salt solution concentration is 30wt%, the molar ratio of ammonia to ammonium salt in the ammonia-ammonium salt mixed solution is 4-5:1, preferably 4:1, and the mass ratio of the ammonia-ammonium salt mixed solution to the copper waste contact body is 1:1. The reaction temperature is 100 degrees Celsius, and the reaction time is 6-8 hours, preferably 8 hours.

[0047] In the secondary dissolution treatment, the ammonia content of the ammonia-ammonium salt mixture is higher than that of the first dissolution treatment. This is because the higher proportion of ammonia can form a stronger alkaline environment, which is conducive to the dissolution of copper, especially for copper compounds that are not easily soluble under acidic conditions (such as CuO, Cu2O, etc.). The presence of NH3 can act as a buffer to stabilize the pH value and avoid side reactions or copper precipitation caused by excessive acidity or alkalinity. Compared with the first dissolution treatment, the copper compound in the secondary dissolution treatment is closer to the core of the material, has a denser texture and more complex compound situation. Therefore, compared with the first dissolution treatment, the treatment liquid of the secondary dissolution treatment needs to have stronger copper dissolution characteristics. However, the ammonia content in the secondary dissolution treatment cannot be too large, for example, greater than the molar ratio of ammonia to ammonium salt 5:1. Since the secondary treatment liquid after the secondary dissolution needs to be treated with ammonia evaporation precipitation, excessive NH3 content will cause the overall acid-base imbalance of the recovered solution, which tends to be alkaline, which is not conducive to the precipitation of precipitation.

[0048] Preferably, during the first dissolution treatment, a stirrer or ultrasonic vibration may be used to promote the complete dissolution of copper in the waste contact body.

[0049] 5) collecting the first and second recovered solutions and performing ammonia evaporation on them to obtain copper precipitate and ammonia gas (which can be recovered and dissolved in ammonia water as a reaction raw material), wherein the copper precipitate can be further subjected to a sintering reaction to obtain copper oxide (as a new catalyst), comprising:

[0050] The first recovery solution obtained by the first dissolution treatment and the second recovery solution obtained by the secondary dissolution treatment are collected and summarized to obtain recovery solutions, and are placed in an ammonia evaporation container. NH4+ salt solution is added to the ammonia evaporation container and mixed evenly. The specific ammonium salt is (NH4)2CO3, and the concentration of the ammonium salt solution is 30wt%. The mass ratio of the added ammonium salt solution to the recovery solution is 1:9, thereby adjusting the acidity and alkalinity of the recovery solution, thereby making the solution acidic during the ammonia evaporation process, which is conducive to the precipitation of copper precipitation. It is worth pointing out that considering the toxicity of NH4+ salt, the amount of NH4+ salt needs to be controlled.

[0051] After filtering the recovered solution, the filtered recovered solution is subjected to ammonia evaporation. The specific ammonia evaporation process includes: heating to 50 degrees Celsius, keeping warm for 9 hours, obtaining copper precipitate basic copper carbonate, and collecting NH3 gas at the same time, which can be received in the ammonia collection device of the system for subsequent dissolution in ammonia water.

[0052] As an alternative embodiment, the solvent in the present application may be an R-OH solvent, and R may be a saturated alkane, an unsaturated alkane, an aromatic hydrocarbon, an ether, or the like.

[0053] As an alternative embodiment, the pairing anions with NH4+ in the ammonium salt may also include Cl-, OH-, HCO3-, etc., and the corresponding copper precipitate may also be a solid mixture of one or more of cupric chloride, cuprous chloride, cupric oxide, cuprous oxide, cupric hydroxide, cuprous hydroxide, and basic copper carbonate.

[0054] Comparative test:

[0055] 60 kg of copper waste contacts (copper content 16 wt%) from the same batch were selected, the waste contacts were fully stirred and mixed, and then divided into 6 portions, each of which weighed 10 kg.

[0056] Example 1 According to the process for extracting copper from polysilicon and organosilicon residual silicon powder provided in the present application above, the process parameters are the most preferred parameters, wherein no stirring or vibration is set during the first and second dissolutions.

[0057] Example 2 According to the process for extracting copper from polysilicon and organosilicon residual silicon powder provided in the present application above, the process parameters are the most preferred parameters, wherein stirring components are set for the first and second dissolutions.

[0058] In Comparative Example 1, no oxygen plasma step is provided between the first dissolution and the second dissolution, and the rest is the same as in Example 1.

[0059] In Comparative Example 2, no additional oxygen was introduced during the first dissolution, and the rest was the same as in Example 1.

[0060] In Comparative Example 3, the ammonia water-ammonium salt mixed solution used in the first dissolution and the second dissolution had a molar ratio of ammonia to ammonium salt of 2:1.

[0061] In Comparative Example 4, no additional NH4+ salt solution was added during the ammonia evaporation process.

[0062]

[0063] Through comparative tests, it can be seen that the process for extracting copper from polysilicon and residual silicon powder of organic silicon provided in the present application can reduce the problem of residual copper metal during the treatment process, reduce the waste in copper element recovery, and improve the treatment efficiency.

[0064] The present invention can achieve the following technical effects:

[0065] 1) Provided is a process for extracting copper from polysilicon and residual silicon powder of organic silicon. The method can reduce the problem of residual copper metal during the treatment process, reduce the waste in copper recovery, and improve the treatment efficiency. The silicon powder after copper recovery can be directly used for casting to form silicon ingots, and at the same time, zero wastewater discharge is achieved in the whole process.

[0066] 2) The remaining solid waste contact body is subjected to plasma treatment. Oxygen plasma treatment increases the surface energy of the particles, improves wettability and adhesion, and the silicon particles treated with oxygen plasma usually show enhanced hydrophilicity, which is beneficial for further reactions in subsequent aqueous dispersions. In addition, after the copper-containing material is treated with oxygen plasma, more copper is oxidized to copper oxide. Since copper oxide is an alkaline oxide, it is easier to react with NH4 + (ammonium ions) react with NH3 (ammonia gas) and then dissolve in the treatment solution to achieve full dissolution of copper. It has certain chemical activity and can react with acidic or alkaline substances under appropriate conditions.

[0067] 3) In the secondary dissolution treatment, the ammonia content of the ammonia-ammonium salt mixture is higher than that of the first dissolution treatment. Compared with the first dissolution treatment, the copper compound in the secondary dissolution treatment is closer to the core of the material, with a denser texture and more complex compound conditions. Therefore, compared with the first dissolution treatment, the treatment liquid of the secondary dissolution treatment needs to have stronger copper dissolution properties. However, the ammonia content in the secondary dissolution treatment cannot be too large, for example, greater than the molar ratio of ammonia to ammonium salt of 5:1. Since the secondary treatment liquid after the secondary dissolution needs to be treated with ammonia evaporation precipitation, excessive NH3 content will cause the overall acid-base imbalance of the recovered solution, which tends to be alkaline, which is not conducive to the precipitation of precipitation.

[0068] 4) A proper amount of ammonium salt is added in the ammonia evaporation step to adjust the acidity and alkalinity of the recovered solution, thereby making the solution acidic during the ammonia evaporation process, which is conducive to the precipitation of copper precipitation.

[0069] 5) Rationally adjust various process parameters to synergistically optimize process effects and extraction efficiency.

[0070] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A process for extracting copper from polysilicon and residual silicon powder of organic silicon, characterized by: The process comprises: using a mixed solution of ammonia water and ammonium salt to dissolve the copper waste contact body, collecting and recovering the solution, and performing ammonia evaporation treatment to obtain a copper-containing precipitate, and sintering the copper-containing precipitate to obtain copper oxide.

2. The process according to claim 1, characterized in that: The ammonium salt is at least one of the Cl-, OH-, CO32-, and HCO3- salts of NH4+.

3. The process according to claim 1, characterized in that: The copper-containing precipitate is a solid mixture of one or more of cupric chloride, cuprous chloride, cupric oxide, cuprous oxide, cupric hydroxide, cuprous hydroxide and basic cupric carbonate.

4. The process according to claim 1, characterized in that: Before using the mixed solution of ammonia water and ammonium salt to dissolve the copper waste contacts, a solid-liquid separation step is also included.

5. The process according to claim 4, characterized in that: The objects of solid-liquid separation are silicon powder and chlorosilane mixture.

6. The process according to claim 4, characterized in that: Solid-liquid separation uses centrifugal drying equipment.

7. The process according to claim 4, characterized in that: Through solid-liquid separation, the content of chlorosilane in silicon powder is controlled within 10%.

8. The process according to claim 4, characterized in that: Through solid-liquid separation, the content of chlorosilane in silicon powder is controlled within 1%.

9. The process according to claim 6, characterized in that: The process parameters of the centrifugal drying equipment include: the rotation speed is 800-1000 rpm, the operating pressure is controlled at 5-150Kpa, and the operating temperature is controlled at 5-300℃.

10. The process according to claim 1, characterized in that: Ammonia evaporation also produces ammonia gas.