ZrNiSn-based Half-Heusler alloy thermoelectric material with intrinsic vacancy and preparation method thereof
By introducing Nb doping and intrinsic structural vacancy in ZrNiSn-based Half-Heusler alloy, the problem of improving thermoelectric superiority is solved, and high ZT value and cost reduction is achieved, which is suitable for commercial applications of medium and high temperature thermoelectric materials.
Patent Information
- Application Number
- CN202411140438.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
Among existing thermoelectric materials, it is difficult to improve the thermoelectric superiority (ZT value), especially because the adjustment of carrier concentration will lead to the mutual coupling of the Seebeck coefficient and the electron thermal conductivity, which limits the thermoelectric performance and production cost of Half-Heusler alloy. .
By introducing Nb doping and intrinsic structural vacancy in ZrNiSn-based Half-Heusler alloy, the vacancy at Ni position is regulated, the thermal conductivity of the lattice is reduced, and the conductivity is improved, the thermoelectric performance is improved, the use of Hf is avoided, and the production is reduced cost.
The high ZT value of Zr0.96Nb0.04Ni0.9Sn alloy was achieved, reaching 1.16, significantly improving the performance of thermoelectric materials and reducing production costs, making it a potential medium and high temperature thermoelectric material suitable for large-scale commercial production and application.
Smart Images

Figure CN118932214A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoelectric materials, and in particular to a ZrNiSn-based Half-Heusler alloy thermoelectric material with intrinsic vacancies and a preparation method thereof. Background Art
[0002] With the increasing environmental pollution and energy crisis, improving energy efficiency has become one of the effective ways to solve environmental and energy problems. Thermoelectric materials are a type of functional materials that use the Seebeck effect and Peltier effect to achieve the mutual conversion between thermal energy and electrical energy. They are expected to be widely used in waste heat recovery power generation and refrigeration fields, thereby improving energy efficiency. In recent years, Half-Heusler alloys with semiconductor characteristics or Seebeck effect have shown good application prospects in the field of temperature difference power generation and can be used as a typical medium and high temperature thermoelectric material.
[0003] The performance of thermoelectric materials mainly depends on their thermoelectric figure of merit ZT. The larger the ZT value, the higher the thermoelectric conversion efficiency. Thermoelectric figure of merit is defined as ZT = α 2 σT / κ, where α is the Seebeck coefficient, σ is the conductivity, and α is the 2 σ can also be defined as the power factor PF, T is the absolute temperature, and κ is the total thermal conductivity, including the lattice (phonon) thermal conductivity κ l and the electronic thermal conductivity κ e (κ=κ l +κ e However, due to these thermoelectric parameters (Seebeck coefficient α, electrical conductivity σ and electronic thermal conductivity κ e ) has a strong dependence on the carrier concentration n and is coupled to each other, that is, obtaining a high conductivity σ by adjusting the carrier concentration n often leads to a low Seebeck coefficient α and a high electronic thermal conductivity κ e Therefore, how to effectively improve the ZT value has always been a difficult problem that has troubled the academic community.
[0004] Half-Heusler compounds are considered to be potential thermoelectric materials with large-scale commercial production and application due to their good high-temperature chemical and thermal stability, excellent mechanical properties, and high high-temperature thermoelectric figure of merit. 0.7 Hf 0.3 NiSn 0.99 Sb 0.01It is the N-type Half-Heusler compound with the best thermoelectric performance. Usually, the Zr position is partially replaced by Hf to reduce the lattice thermal conductivity. However, the optimal doping amount of Hf in this system is between 0.3 and 0.7. Excessive use of Hf will increase the production cost of thermoelectric materials and limit their practical application. If the optimal doping amount of Hf is not between 0.3 and 0.7, its thermoelectric performance will be poor. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a ZrNiSn-based Half-Heusler alloy thermoelectric material with intrinsic vacancies and a preparation method and application thereof. The ZrNiSn-based Half-Heusler alloy thermoelectric material provided by the present invention can effectively improve the thermoelectric performance of the ZrNiSn-based Half-Heusler thermoelectric material, effectively avoid the use of Hf, and reduce production costs.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a ZrNiSn-based Half-Heusler alloy thermoelectric material with intrinsic vacancies, the chemical composition of which is Zr 0.96 Nb 0.04 Ni 1-x Sn, where the value range of x is 0≤x≤0.2.
[0008] Preferably, the value of x is 0, 0.05, 0.1, 0.15 or 0.2.
[0009] The present invention also provides a method for preparing the above-mentioned ZrNiSn-based Half-Heusler alloy thermoelectric material, comprising the following steps:
[0010] Corresponding to the chemical element composition of the ZrNiSn-based Half-Heusler thermoelectric material, the alloy raw material is smelted under protective atmosphere conditions to obtain an alloy ingot;
[0011] Grinding and drying the alloy ingot in sequence to obtain alloy powder;
[0012] The alloy powder is subjected to spark plasma sintering to obtain the ZrNiSn-based Half-Heusler alloy thermoelectric material.
[0013] Preferably, the protective atmosphere is argon; the smelting is magnetic suspension smelting; the temperature of the magnetic suspension smelting is 1500-2000°C, the holding time is 1-5 minutes, and the pressure of the argon gas is 10 4 ~10 5Pa; the number of magnetic levitation melting is 3 to 6 times.
[0014] Preferably, the grinding process is performed until the particle size of the material is 0.5-2 μm.
[0015] Preferably, the grinding comprises firstly grinding the ingot into powder with a particle size of 0.1 to 1 mm using a mortar; and then performing wet ball milling in an argon atmosphere.
[0016] Preferably, the medium for wet ball milling is anhydrous ethanol, the ball-to-material ratio is 10:1-20:1, the rotation speed is 200-600 r / min, and the wet ball milling time is 5-20 h.
[0017] Preferably, the temperature of the spark plasma sintering is 900-1000° C., the pressure of the spark plasma sintering is 80-100 MPa, and the holding time is 5-20 min.
[0018] Preferably, the alloy raw material includes Zr particles, Nb particles, Ni particles and Sn particles.
[0019] Preferably, the Zr particles, Nb particles, Ni particles and Sn particles are independently small particles of 1×2 mm to 2×5 mm.
[0020] The present invention provides a ZrNiSn-based Half-Heusler alloy thermoelectric material with intrinsic vacancies, the chemical composition of which is Zr 0.96 Nb 0.04 Ni 1-x Sn, wherein the value range of x is 0≤x≤0.2. The present invention selects ZrNiSn alloy as the master alloy, and by regulating the intrinsic structural vacancies at the Ni position and replacing the Nb at the Zr position, Nb doping can also effectively stabilize the existence of the intrinsic structural vacancies; in addition, Nb doping and intrinsic structural vacancies can significantly improve the electrical conductivity, and the introduction of intrinsic structural vacancies and Nb doping can cause large lattice distortion field and mass field fluctuations, effectively scatter phonons, and reduce lattice thermal conductivity, thereby improving the thermoelectric performance of ZrNiSn-based Half-Heusler thermoelectric materials, effectively avoiding the use of Hf, and reducing production costs.
[0021] The data of the embodiment show that: through XRD detection, a single-phase Zr 0.96 Nb 0.04 Ni 1-x Sn (x = 0, 0.05, 0.1, 0.15 or 0.2) thermoelectric material, in which Nb doping can effectively improve the stability of intrinsic structure vacancies in the matrix. Thermoelectric test results show that when the Nb doping content is 0.04 and the intrinsic structure Ni vacancy content is 0.1, Zr 0.96 Nb 0.04 Ni0.9 The lattice thermal conductivity of Sn alloy is as low as 1.19mW / mK 2 , and finally its ZT value is as high as 1.16, indicating that the Half-Heusler thermoelectric material prepared by the present invention is a potential medium- and high-temperature thermoelectric material that can be commercially produced and applied on a large scale.
[0022] The present invention also provides a method for preparing the ZrNiSn-based Half-Heusler alloy thermoelectric material, comprising the following steps: corresponding to the chemical element composition of the ZrNiSn-based Half-Heusler thermoelectric material, melting the alloy raw material under protective atmosphere conditions to obtain an alloy ingot; grinding and drying the alloy ingot in sequence to obtain an alloy powder; and performing discharge plasma sintering on the alloy powder to obtain the ZrNiSn-based Half-Heusler alloy thermoelectric material. The method has the advantages of short process, few steps, and easy control of intrinsic structural vacancies. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 XRD diagrams of samples of Examples 1 to 5;
[0024] Figure 2 TEM images of samples of Examples 1 to 5;
[0025] Figure 3 The electrical performance diagrams of the samples of Examples 1 to 5;
[0026] Figure 4 The Seebeck coefficient, conductivity and power factor diagram of the samples of Examples 1 to 5;
[0027] Figure 5 Graph showing the ZT values and ZT average values of samples of Examples 1 to 5 and the Hf-doped sample of the comparative example. DETAILED DESCRIPTION
[0028] The present invention provides a ZrNiSn-based Half-Heusler alloy thermoelectric material with intrinsic vacancies, the chemical composition of which is Zr 0.96 Nb 0.04 Ni 1-x Sn, where the value range of x is 0≤x≤0.2.
[0029] In the present invention, the value of x is preferably 0, 0.05, 0.1, 0.15 or 0.2.
[0030] The present invention also provides a method for preparing the ZrNiSn-based Half-Heusler alloy thermoelectric material described in the above technical solution, comprising the following steps:
[0031] Corresponding to the chemical element composition of the ZrNiSn-based Half-Heusler thermoelectric material, the alloy raw material is smelted under protective atmosphere conditions to obtain an alloy ingot;
[0032] Grinding and drying the alloy ingot in sequence to obtain alloy powder;
[0033] The alloy powder is subjected to spark plasma sintering to obtain the ZrNiSn-based Half-Heusler alloy thermoelectric material.
[0034] The invention corresponds to the chemical element composition of the ZrNiSn-based Half-Heusler thermoelectric material, and melts the alloy raw material under protective atmosphere conditions to obtain an alloy ingot.
[0035] In the present invention, the alloy raw materials preferably include Zr particles, Nb particles, Ni particles and Sn particles; the Zr particles, Nb particles, Ni particles and Sn particles are independently preferably small particles of 1×2 mm to 2×5 mm.
[0036] In the present invention, the protective atmosphere is preferably argon; the smelting is preferably magnetic suspension smelting; the temperature of the magnetic suspension smelting is preferably 1500-2000°C, more preferably 1600-1800°C; the heating rate to the temperature of the magnetic suspension smelting is preferably 1000-3000°C / min, more preferably 1500-2500°C / min; the holding time is preferably 1-5min, more preferably 3-5min; during the magnetic suspension smelting, the pressure of argon is preferably 10 4 ~10 5 Pa, more preferably 5×10 4 Pa; the number of magnetic levitation melting is preferably 3 to 6 times, more preferably 4 to 5 times.
[0037] After obtaining the alloy ingot, the present invention grinds and dries the alloy ingot in sequence to obtain alloy powder.
[0038] In the present invention, the grinding is preferably performed until the particle size of the material is preferably 0.5 to 2 μm. In the present invention, the grinding is preferably performed by first using a mortar to coarsely grind the ingot into a powder with a particle size of 0.1 to 1 mm; then wet ball milling is performed under an argon atmosphere; the medium for wet ball milling is preferably anhydrous ethanol, the ball-to-material ratio is preferably 10 to 20:1, more preferably 15:1, the rotation speed is preferably 200 to 600 r / min, more preferably 300 to 500 r / min; the time for wet ball milling is preferably 5 to 20 h, more preferably 10 to 15 h.
[0039] In the present invention, after the grinding, it is preferred to further include suction filtration.
[0040] In the present invention, the drying is preferably natural drying, and the natural drying step is preferably to dry the filtered powder naturally in a glove box for 12 to 48 hours, more preferably 12 to 24 hours.
[0041] After obtaining the alloy powder, the present invention performs spark plasma sintering on the alloy powder to obtain the ZrNiSn-based Half-Heusler alloy thermoelectric material.
[0042] In the present invention, the temperature of the spark plasma sintering is preferably 900-1000°C, more preferably 950°C; the heating rate to the temperature of the spark plasma sintering is preferably 100-300°C / min, more preferably 150-250°C / min; the pressure of the spark plasma sintering is preferably 80-100MPa, more preferably 90MPa, and the holding time is preferably 5-20min, more preferably 10-15min.
[0043] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0044] Example 1
[0045] A ZrNiSn-based Half-Heusler thermoelectric material with the chemical formula Zr 0.96 Nb 0.04 Ni 1-x Sn, wherein x is selected from 0.
[0046] The preparation method is as follows:
[0047] Material selection: Zr, Nb, Ni, Sn are selected as small particles with a diameter × length of 2 × 5mm and a purity of 99.9%.
[0048] In the glove box, follow the Zr 0.96 Nb 0.04 NiSn raw material ratio, Zr, Nb, Ni, Sn particles are placed in a magnetic suspension smelting furnace.
[0049] Melting: In an argon protective atmosphere (pressure of 0.07 MPa), the temperature was raised to 1700°C and kept for 3 minutes. The melting was repeated 4 times to obtain an alloy ingot.
[0050] Ball milling and filtration: First, the alloy ingot was coarsely ground into powder with a particle size of 0.5 mm using a mortar, and then wet ball milled in an argon atmosphere. The wet ball milling medium was anhydrous ethanol, the ball-to-material ratio was 15:1, the rotation speed was 500 r / min, and the ball milling time was 10 h.
[0051] After wet ball milling, the alloy powder with a particle size of ~1μm was obtained by filtration.
[0052] Drying treatment: The filtered powder was naturally dried in a glove box for 24 hours.
[0053] Sintering: The dried alloy powder was subjected to spark plasma sintering at a sintering temperature of 1000°C, a sintering pressure of 100 MPa, and a holding time of 15 min to obtain a ZrNiSn-based Half-Heusler alloy thermoelectric material, recorded as sample-1.
[0054] Example 2
[0055] The only difference from Example 1 is that the thermoelectric material, the chemical formula is Zr 0.96 Nb 0.04 Ni 1-x Sn, x is 0.05, and the product is recorded as sample-2.
[0056] Example 3
[0057] The only difference from Example 1 is that the thermoelectric material, the chemical formula is Zr 0.96 Nb 0.04 Ni 1-x Sn, x is 0.1, and the product is recorded as sample-3.
[0058] Example 4
[0059] The only difference from Example 1 is that the thermoelectric material, the chemical formula is Zr 0.96 Nb 0.04 Ni 1-x Sn, x is 0.15 and the product is recorded as sample-4.
[0060] Example 5
[0061] The only difference from Example 1 is that the thermoelectric material, the chemical formula is Zr 0.96 Nb 0.04 Ni 1-x Sn, x is 0.2, and the product is recorded as sample-5.
[0062] The XRD patterns of the samples in Examples 1 to 5 are as follows: Figure 1 As shown, from Figure 1 It can be seen that Zr 0.96 Nb 0.04 Ni 1-x There are fewer impurities in the Sn (x=0, 0.05, 0.1, 0.15, 0.2) samples.
[0063] TEM images of samples of Examples 1 to 5 are as follows: Figure 2 As shown, from Figure 2It can be seen that the intrinsic Ni structural vacancies were successfully introduced into the matrix, and the intrinsic structural vacancies did not change the crystal structure of the ZrNiSn sample.
[0064] The present invention uses an electrical comprehensive test system to test the electrical properties of samples in Examples 1 to 5, and uses a laser thermal conductivity meter to measure the thermal conductivity of samples in Examples 1 to 5 above room temperature. The results are as follows: Figure 3 As shown, from Figure 3 It can be seen that the introduction of Nb doping and intrinsic Ni structural vacancies can effectively improve the conductivity of the sample, and its Seebeck coefficient has not deteriorated significantly.
[0065] The Seebeck coefficient, conductivity and power factor of the samples of Examples 1 to 5 are shown in the figure below: Figure 4 shown; from Figure 4 It can be seen that when the Nb doping content is 0.04 and the intrinsic structure Ni vacancy content is 0.1, Zr 0.96 Nb 0.04 Ni 0.9 The lattice thermal conductivity of Sn alloy is as low as 1.19mW / mK 2 , thus effectively replacing the use of Hf.
[0066] The ZT values and ZT average values of the samples in Examples 1 to 5 and the Hf-doped samples in the comparative example are as follows: Figure 5 As shown. Figure 5 It can be seen that when the Nb doping content is 0.04 and the intrinsic structure Ni vacancy content is 0.1, Zr 0.96 Nb 0.04 Ni 0.9 The maximum ZT value of the Sn alloy is 1.16 at 1073K, which is the highest ZT value among the single-doped samples and is 99% higher than that of the ZrNiSn matrix. It can effectively avoid the use of Hf and effectively reduce the production cost.
[0067] Comparative Example 1
[0068] The sample is Zr 0.3 Hf 0.65 Ta 0.05 NiSn;
[0069] Comparative Example 2
[0070] The sample is Zr 0.4 Hf 0.6 NiSn 0.98 Sb 0.02 ;
[0071] Comparative Example 3
[0072] The sample is Zr 0.68 Hf 0.3 Ta0.02 NiSn;
[0073] Comparative Example 4
[0074] The sample is Zr 0.2 Hf 0.8 NiSn 0.985 Sb 0.015 ;
[0075] Comparative Example 5
[0076] The sample is Zr 0.25 Hf 0.75 NiSn 0.99 Sb 0.001 .
[0077] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A ZrNiSn-based Half-Heusler alloy thermoelectric material with intrinsic vacancies, characterized in that: The chemical composition is Zr 0.96 Nb 0.04 Ni 1-x Sn, where the value range of x is 0≤x≤0.
2.
2. The ZrNiSn-based Half-Heusler alloy thermoelectric material according to claim 1, characterized in that: The value of x is 0, 0.05, 0.1, 0.15 or 0.
2.
3. The method for preparing the ZrNiSn-based Half-Heusler alloy thermoelectric material according to claim 1 or 2, characterized in that: The following steps are involved: Corresponding to the chemical element composition of the ZrNiSn-based Half-Heusler thermoelectric material, the alloy raw material is smelted under protective atmosphere conditions to obtain an alloy ingot; Grinding and drying the alloy ingot in sequence to obtain alloy powder; The alloy powder is subjected to spark plasma sintering to obtain the ZrNiSn-based Half-Heusler alloy thermoelectric material.
4. The preparation method according to claim 3, characterized in that: The protective atmosphere is argon; the smelting is magnetic suspension smelting; the temperature of the magnetic suspension smelting is 1500-2000°C, the insulation time is 1-5min, and the pressure of argon is 10 4 ~10 5 Pa; the number of magnetic levitation melting is 3 to 6 times.
5. The preparation method according to claim 3, characterized in that: The grinding step is performed until the particle size of the material is 0.5 to 2 μm.
6. The preparation method according to claim 5, characterized in that: The grinding process firstly grinds the ingot into powder with a particle size of 0.1 to 1 mm using a mortar, and then performs wet ball milling in an argon atmosphere.
7. The preparation method according to claim 6, characterized in that: The medium of the wet ball milling is anhydrous ethanol, the ball-to-material ratio is 10:1-20:1, the rotation speed is 200-600 r / min, and the wet ball milling time is 5-20 hours.
8. The preparation method according to claim 3, characterized in that: The temperature of the spark plasma sintering is 900-1000° C., the pressure of the spark plasma sintering is 80-100 MPa, and the heat preservation time is 5-20 minutes.
9. The preparation method according to claim 3, characterized in that: The alloy raw materials include Zr particles, Nb particles, Ni particles and Sn particles.
10. The preparation method according to claim 9, characterized in that: The Zr particles, Nb particles, Ni particles and Sn particles are independently small particles of 1×2 mm to 2×5 mm.
Citation Information
Cited By
Smelting method of Heusler alloy Co2MnAl
CN120989386A