Au-coated H-TiO2 Janus structure SERS (Surface Enhanced Raman Scattering) substrate as well as preparation method and application thereof

By preparing Au@H-TiO2 Janus structured SERS substrates, the interaction between the analyte and the substrate was enhanced using sodium citrate reduction and a one-step hydrothermal method. This solved the problem of weak adsorption capacity of traditional SERS substrates and enabled the detection of low-concentration pollutants with high sensitivity and stability.

CN118937302APending Publication Date: 2024-11-12XUZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411020967.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing SERS substrates have weak adsorption capacity for pollutants, making it difficult to achieve rapid detection of low-concentration pollutants and limiting their application in real life.

Method used

Gold nanoparticles were prepared using a SERS substrate with an Au@H-TiO2 Janus structure via sodium citrate reduction, and hollow titanium dioxide was prepared by a one-step hydrothermal method. The interfacial tension was used to form the Au@H-TiO2 Janus structure, which enhanced the interaction between the analyte and the substrate.

Benefits of technology

It improves the sensitivity and stability of SERS detection, and can be used multiple times to meet the needs of rapid on-site detection of low-concentration pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937302A_ABST
    Figure CN118937302A_ABST
Patent Text Reader

Abstract

The invention discloses an SERS (Surface Enhanced Raman Scattering) substrate with an Au-coated H-TiO2 Janus structure as well as a preparation method and application of the SERS substrate with the Au-coated H-TiO2 Janus structure. Gold nanoparticles are prepared by adopting a sodium citrate reduction method, and a hollow spherical porous titanium dioxide material is synthesized by adopting a one-step hydrothermal method. A piranha solution is used for modifying a silicon wafer, a hollow titanium dioxide solution is dropwise added to a hydrophilic silicon wafer carrier, and a compact hollow titanium dioxide film is formed after an organic solvent is evaporated. And enabling the gold nanoparticles to form a regular gold film between an organic phase and an inorganic phase by using interfacial tension, and then transferring the gold film to the hollow titanium dioxide film, thereby obtaining the Au-coated H-TiO2Janus nanostructure. The used material is the hollow spherical titanium dioxide with the porous surface, a Janus structure enables half of the surface of the titanium dioxide to be modified with gold nanoparticles and half of the surface of the titanium dioxide to be not modified with gold nanoparticles, and the titanium dioxide can rapidly move under irradiation of Raman laser, so that pollutants can be fully adsorbed in the detection process, and the detection sensitivity of the substrate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to Au@H-TiO 2 The invention discloses a Janus structure SERS substrate, a preparation method and an application thereof, belonging to the field of nanocomposite materials, and specifically relates to a SERS detection technology for pollutants in the environment. Background Art

[0002] The United Nations Water Report pointed out that 2 billion people in the world do not have safe drinking water, accounting for about 26% of the world's population. Long-term drinking of contaminated water will lead to chronic poisoning, and severe cases may induce cancer. At present, traditional analytical techniques have the disadvantages of expensive equipment, complex operation, and complex sample pretreatment, which limit their application in real life. Therefore, the development of a water quality detection technology with high sensitivity, good reproducibility, simple operation, and strong practicality is of great significance for the rapid and sensitive detection of pollutants. Surface enhanced Raman scattering spectroscopy (SERS) is a spectral analysis technology for detecting trace targets. It has the advantages of high sensitivity, fast detection speed, low water interference, and no damage to samples. Since the gap connection between metal nanostructures or the "hot spots" generated by the nano gap can cause strong local electromagnetic field enhancement, it has significant advantages in the analysis of low-concentration pollutants.

[0003] Since the discovery of SERS technology, researchers have focused on preparing various SERS substrates to effectively improve SERS signals. At present, substrate materials with high SERS performance have been successfully constructed through magnetron sputtering, ion beam lithography, atomic layer deposition and other technologies. However, due to the weak adsorption capacity of the substrate for the analyte, most target molecules find it difficult to reach the plasma resonance area on the substrate surface, making it difficult for SERS detection to meet the needs of rapid on-site detection of low-concentration pollutants, greatly reducing the application of SERS technology in the field of pollutant detection in real life. Summary of the invention

[0004] Based on this, the present invention provides an Au@H-TiO 2 A Janus structure SERS substrate, preparation method and application are provided to solve the problem in the prior art that the SERS substrate has a weak adsorption capacity for pollutants and is difficult to achieve low-concentration detection.

[0005] To achieve the above object, the present invention provides an Au@H-TiO 2 The preparation method of the Janus structure SERS substrate is innovative in that it includes the following steps:

[0006] Step S1: Preparation of gold nanoparticles Au NPs

[0007] HAuCl with a mass ratio of 0.5%-1.5% 4·3H 2 O was dissolved in deionized water to obtain a solution, in which HAuCl 4 ·3H 2 The volume ratio of O and deionized water is 0.15-1.5:90-110. After the above solution is heated to boiling, 0.5%-1.5% sodium citrate is added dropwise, wherein HAuCl 4 ·3H 2 The volume ratio of O and sodium citrate is 0.15-1.5:2-3, and heating is stopped when the solution turns wine red to obtain gold nanoparticles Au NPs for use;

[0008] Step S2: Preparation of hollow titanium dioxide H-TiO2

[0009] Anhydrous ethanol, polyvinyl pyrrolidone aqueous solution, hydrochloric acid and titanium tetrafluoride aqueous solution in a volume ratio of 25-30: 3-5: 0.2-0.3: 2-3 were mixed evenly and placed in a polytetrafluoroethylene liner. After standing for one hour, the suspension was heated in a reactor at 160-200°C for 3 hours. Finally, the product was centrifuged and washed with water for 3 times and dried to obtain titanium dioxide H-TiO2 with a hollow structure.

[0010] Step S3: Au@H-TiO 2 Preparation of Janus structure SERS substrate

[0011] First, the silicon wafer needs to be modified. The silicon wafer is cut into equal-sized squares and cleaned with ethanol and deionized water. Then, the cleaned silicon wafer is placed in a boiling piranha solution for 20-40 minutes. After being taken out, it is ultrasonically cleaned six times with deionized water, each time for 15 minutes.

[0012] Take 1-3 mg of hollow titanium dioxide H-TiO in step S2 2 , ultrasonically dispersed in 10-14 ml of anhydrous ethanol, dropped on the modified silicon wafer, placed at room temperature, and after the anhydrous ethanol on the surface evaporated, a hollow titanium dioxide film was obtained;

[0013] Take 5-7mL of gold nanoparticles Au NPs in step S1, drop 1-2mL of cyclohexane to form a water / cyclohexane immiscible interface between the two phases, add anhydrous ethanol dropwise until golden mirror reflection appears, immerse the silicon wafer carrying the hollow titanium dioxide film in the nanoparticle monolayer film, and slowly withdraw it after the silicon wafer and the gold film on the interface are completely attached. After the cyclohexane evaporates naturally at room temperature, 2 The silicon wafer was calcined in a tube furnace at 400-500°C for 1-3h under protective gas, and the mixture was calcined. The product was peeled off from the silicon wafer substrate to obtain Au@H-TiO 2 Janus structured nanocomposites.

[0014] Preferably, in step S1, HAuCl 4 ·3H 2 O mass ratio is 1%, take 1 ml, the above HAuCl 4 ·3H 2 The amount of deionized water solvent used is 100 ml, and 3 ml of sodium citrate is added at a mass ratio of 1%.

[0015] Preferably, in step S2, the amount of anhydrous ethanol used is 27.6 ml, the amount of polyvinyl pyrrolidone aqueous solution used is 4 ml, the amount of hydrochloric acid used is 0.25 ml, and the amount of titanium tetrafluoride used is 2.5 ml.

[0016] Preferably, the concentration of the polyvinyl pyrrolidone aqueous solution is 9.75 mg / mL, the concentration of the hydrochloric acid is 0.1 M, and the concentration of the titanium tetrafluoride aqueous solution is 0.04 M.

[0017] Preferably, in step S3, the size of the silicon wafer is 1×1 cm; the piranha solution is prepared from concentrated sulfuric acid and 30% by mass hydrogen peroxide, the volume ratio of concentrated sulfuric acid to hydrogen peroxide is 7:3, and the silicon wafer is boiled in the piranha solution for 30 minutes.

[0018] Preferably, in step S3, the amount of hollow titanium dioxide used is 2 mg, the concentration of hollow titanium dioxide is 0.003M-0.004M, the amount of anhydrous ethanol used is 12 ml, the ultrasonic time is 10 min, and the amount added to each silicon wafer is 200 μL.

[0019] Preferably, in step S3, the amount of gold nanoparticles Au NPs used is 6 ml, the amount of cyclohexane used is 1.5 ml, and when golden mirror reflection appears at the water / cyclohexane immiscible interface, the dropwise addition of anhydrous ethanol is stopped.

[0020] Preferably, in step S3, Au@H-TiO 2 The silicon wafer was calcined in a tube furnace at a temperature of 500°C for 2 hours. N 2 / H 2 =90 / 10 as protective gas.

[0021] Au@H-TiO 2 Janus structure SERS substrate, using Au@H-TiO 2 The preparation method of Janus structure SERS substrate was used to prepare Au@H-TiO 2 Janus structure SERS substrate.

[0022] Au@H-TiO 2Application of Janus structure SERS substrate, application of Au@H-TiO 2 Janus structure SERS substrate, Au@H-TiO 2 Janus structure SERS substrate is used in SERS detection.

[0023] The advantages of the present invention are:

[0024] The Au@H-TiO 2 Janus structure SERS substrate, preparation method and application, Au NPs are reduced by sodium citrate, which is simple to operate and has high repetition rate; H-TiO prepared by one-step hydrothermal method 2 The size is uniform, the morphology is regular, it is a spherical hollow structure, the surface has uniform pore distribution, and has a large specific surface area; the prepared composite nano-substrate has high stability, the components are well combined, the SERS detection sensitivity is high, the stability is good, and it can be recycled many times.

[0025] Au@H-TiO 2 The Janus structure SERS substrate can strengthen the interaction between the analyte and the SERS substrate through adsorption, thereby enhancing the sensitivity of SERS detection. Due to the excellent photocatalytic properties of titanium dioxide, pollutants adsorbed on the surface during the detection process can be degraded, thereby solving the problem that the traditional SERS substrate can only be used once, and can meet the needs of rapid on-site detection of low-concentration pollutants in the environment.

[0026] The present invention adopts sodium citrate reduction method to prepare gold nanoparticles, and uses a one-step hydrothermal method to synthesize hollow spherical porous titanium dioxide material. The silicon wafer is modified with piranha solution, and the hollow titanium dioxide solution is dripped on the hydrophilic silicon wafer carrier, and a dense hollow titanium dioxide film is formed after the organic solvent evaporates. The interfacial tension is used to make the gold nanoparticles form a regular gold film between the organic phase and the inorganic phase, and then the gold film is transferred to the hollow titanium dioxide film to obtain Au@H-TiO 2 Janus nanostructure. The material used in the present invention is a hollow spherical titanium dioxide with a porous surface. The Janus structure makes the titanium dioxide surface half modified with gold nanoparticles and half without. It can move quickly under the irradiation of Raman laser, so that pollutants can be fully adsorbed during the detection process, thereby improving the detection sensitivity of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0028] Figure 1 is a scanning electron microscope image of Au NPs in Example 1 of the present invention;

[0029] Figure 2 It is H-TiO in Example 1 of the present invention. 2 Scanning electron microscope image of

[0030] Figure 3 It is H-TiO in Example 1 of the present invention. 2 Transmission electron microscope image of

[0031] Figure 4 The Au@H-TiO 2 Scanning electron microscope image of Janus structure SERS substrate;

[0032] Figure 5 The Au@H-TiO 2 Raman spectra of R6G detected by Janus structure SERS substrate under laser irradiation at different times;

[0033] Figure 6 The Au@H-TiO 2 Detection uniformity of R6G on Janus structure SERS substrate.

[0034] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0035] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0036] The technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0037] Au@H-TiO 2 The preparation method of the Janus structure SERS substrate comprises the following steps:

[0038] Step S1: Preparation of gold nanoparticles Au NPs

[0039] HAuCl with a mass ratio of 0.5%-1.5% 4 ·3H 2 O was dissolved in deionized water to obtain a solution, in which HAuCl 4 ·3H 2The volume ratio of O and deionized water is 0.15-1.5:90-110. After the above solution is heated to boiling, 0.5%-1.5% sodium citrate is added dropwise, wherein HAuCl 4 ·3H 2 The volume ratio of O and sodium citrate is 0.15-1.5:2-3, and heating is stopped when the solution turns wine red to obtain gold nanoparticles Au NPs for use;

[0040] Step S2: Preparation of hollow titanium dioxide H-TiO2

[0041] Anhydrous ethanol, polyvinyl pyrrolidone aqueous solution, hydrochloric acid and titanium tetrafluoride aqueous solution in a volume ratio of 25-30: 3-5: 0.2-0.3: 2-3 were mixed evenly and placed in a polytetrafluoroethylene liner. After standing for one hour, the suspension was heated in a reactor at 160-200°C for 3 hours. Finally, the product was centrifuged and washed with water for 3 times and dried to obtain titanium dioxide H-TiO2 with a hollow structure.

[0042] Step S3: Au@H-TiO 2 Preparation of Janus structure SERS substrate

[0043] First, the silicon wafer needs to be modified. The silicon wafer is cut into equal-sized squares and cleaned with ethanol and deionized water. Then, the cleaned silicon wafer is placed in a boiling piranha solution for 20-40 minutes. After being taken out, it is ultrasonically cleaned six times with deionized water, each time for 15 minutes.

[0044] Take 1-3 mg of hollow titanium dioxide H-TiO in step S2 2 , ultrasonically dispersed in 10-14 ml of anhydrous ethanol, dropped onto the modified silicon wafer, placed at room temperature, and after the anhydrous ethanol on the surface evaporated, a hollow titanium dioxide film was obtained;

[0045] Take 5-7mL of gold nanoparticles Au NPs in step S1, drop 1-2mL of cyclohexane to form a water / cyclohexane immiscible interface between the two phases, add anhydrous ethanol dropwise until golden mirror reflection appears, immerse the silicon wafer carrying the hollow titanium dioxide film in the nanoparticle monolayer film, and slowly withdraw it after the silicon wafer and the gold film on the interface are completely attached. After the cyclohexane evaporates naturally at room temperature, 2 The silicon wafer was calcined in a tube furnace at 400-500°C for 1-3h under protective gas, and the mixture was calcined. The product was peeled off from the silicon wafer substrate to obtain Au@H-TiO 2 Janus structured nanocomposites.

[0046] Au NPs were reduced by sodium citrate, which is simple to operate and has a high reproducibility. H-TiO 2 The size is uniform, the morphology is regular, it is a spherical hollow structure, the surface has a uniform distribution of pores, and has a large specific surface area; the prepared composite nano-substrate has high stability, the components are well combined, the SERS detection sensitivity is high, the stability is good, and it can be recycled many times. Au@H-TiO 2 The Janus structure SERS substrate can strengthen the interaction between the analyte and the SERS substrate through adsorption, thereby enhancing the sensitivity of SERS detection. Due to the excellent photocatalytic properties of titanium dioxide, pollutants adsorbed on the surface during the detection process can be degraded, thereby solving the problem that the traditional SERS substrate can only be used once, and can meet the needs of rapid on-site detection of low-concentration pollutants in the environment.

[0047] HAuCl in step S1 above 4 ·3H 2 O mass ratio is 1%, take 1 ml, the above HAuCl 4 ·3H 2 The amount of deionized water solvent is 100 ml, and 3 ml of sodium citrate is added at a mass ratio of 1%. In step S2, the amount of anhydrous ethanol is 27.6 ml, the amount of polyvinyl pyrrolidone aqueous solution is 4 ml, the amount of hydrochloric acid is 0.25 ml, the amount of titanium tetrafluoride is 2.5 ml, the concentration of polyvinyl pyrrolidone aqueous solution is 9.75 mg / mL, the concentration of hydrochloric acid is 0.1 M, and the concentration of titanium tetrafluoride aqueous solution is 0.04 M.

[0048] In the above step S3, the size of the silicon wafer is 1×1 cm; the piranha solution is prepared from concentrated sulfuric acid and 30% hydrogen peroxide, the volume ratio of concentrated sulfuric acid to hydrogen peroxide is 7:3, and the silicon wafer is boiled in the piranha solution for 30 minutes. The amount of hollow titanium dioxide is 2 mg, the concentration of hollow titanium dioxide is 0.003M-0.004M, the amount of anhydrous ethanol is 12 ml, the ultrasonic time is 10 min, and the amount added to each silicon wafer is 200 μL. In step S3, the amount of gold nanoparticles Au NPs is 6 ml, and the amount of cyclohexane is 1.5 ml. When a golden mirror reflection appears at the water / cyclohexane immiscible interface, stop adding anhydrous ethanol. Step S3 contains Au@H-TiO 2 The silicon wafer was calcined in a tube furnace at a temperature of 500°C for 2 hours. N 2 / H 2 =90 / 10 as protective gas.

[0049] Au@H-TiO 2Janus structure SERS substrate, using Au@H-TiO 2 The preparation method of Janus structure SERS substrate was used to prepare Au@H-TiO 2 Janus structure SERS substrate.

[0050] Au@H-TiO 2 Application of Janus structure SERS substrate, application of Au@H-TiO 2 Janus structure SERS substrate, Au@H-TiO 2 Janus structure SERS substrate is used in SERS detection.

[0051] Embodiment 1:

[0052] Step S1: Synthesis of gold nanoparticles Au NPs

[0053] Reduction of HAuCl by Au NPs using sodium citrate 4 ·3H 2 O method. Specifically, add 100 ml of deionized water and 1 ml of 1% HAuCl in a 100 ml round-bottom flask. 4 ·3H 2 O, stir magnetically at 120°C and 350rpm until boiling, quickly add 3ml of 1% sodium citrate, and stop heating when the color turns into a stable wine red. The prepared gold nanoparticles Au NPs are 16nm.

[0054] Step S2: Hollow Titanium Dioxide H-TiO 2 Preparation

[0055] 27.6 mL of anhydrous ethanol, 4 mL of polyvinyl pyrrolidone aqueous solution with a concentration of 9.75 mg / mL, 250 μL of 0.1 M hydrochloric acid HCl, and 2.5 mL of 0.04 M titanium tetrafluoride aqueous solution TiF 4 The aqueous solution was mixed and placed in a polytetrafluoroethylene reactor and heated at 180 °C for 3 hours. Finally, the product was centrifuged and washed with water 3 times to obtain a hollow structure TiO 2 .

[0056] Step S3: Au@H-TiO 2 Preparation of Janus structure SERS substrate

[0057] Place the silicon wafer in piranha solution (H 2 SO 4 :H 2 O 2=7:3) for 30 min to make it a hydrophilic carrier. The modified silicon wafer was ultrasonically cleaned in deionized water for six times, each time for 15 min. 2 mg of 0.0039 M TiO2 suspension was evenly dropped on the modified silicon wafer and dried to obtain a dense hollow TiO 2 film.

[0058] Add 1.5 mL of cyclohexane to 6 mL of gold nanoparticles Au NPs, and then add anhydrous ethanol dropwise until a golden mirror reflection appears at the organic / inorganic interface. Use tweezers to slowly immerse the silicon wafer in the mixed solution, and carefully take it out after the silicon wafer and the gold film are completely attached. Place the composite material at room temperature to allow the cyclohexane on the gold film surface to evaporate naturally, and you can get Au@TiO 2 Jans Structural Composites.

[0059] Embodiment 2:

[0060] Step S1: Synthesis of gold nanoparticles Au NPs

[0061] Reduction of HAuCl by Au NPs using sodium citrate 4 ·3H 2 O method. Specifically, add 100 ml of deionized water and 1 ml of 1% HAuCl in a 100 ml round-bottom flask. 4 ·3H 2 O, stir magnetically at 120°C and 350rpm until boiling, quickly add 1ml of 1% sodium citrate, and stop heating when the color turns into a stable wine red. The prepared gold nanoparticles Au NPs are 16nm.

[0062] Step S2: Hollow Titanium Dioxide H-TiO 2 Preparation

[0063] 27.6 mL of anhydrous ethanol, 4 mL of polyvinyl pyrrolidone aqueous solution with a concentration of 9.75 mg / mL, 250 μL of 0.1 M hydrochloric acid HCl, and 2.5 mL of 0.04 M titanium tetrafluoride aqueous solution TiF 4 The aqueous solution was mixed and placed in a polytetrafluoroethylene reactor and heated at 180 °C for 3 hours. Finally, the product was centrifuged and washed with water 3 times to obtain a hollow structure TiO 2 .

[0064] Step S3: Au@H-TiO 2 Preparation of Janus structure SERS substrate

[0065] Place the silicon wafer in piranha solution (H 2 SO 4 :H 2 O2 =7:3) for 30 min to make it a hydrophilic carrier. The modified silicon wafer was ultrasonically cleaned in deionized water for six times, each time for 15 min. 2 mg of 0.0039 M TiO2 suspension was evenly dropped on the modified silicon wafer and dried to obtain a dense hollow TiO 2 film.

[0066] Add 1.5 mL of cyclohexane to 6 mL of gold nanoparticles Au NPs, and then add anhydrous ethanol dropwise until a golden mirror reflection appears at the organic / inorganic interface. Use tweezers to slowly immerse the silicon wafer in the mixed solution, and carefully take it out after the silicon wafer and the gold film are completely attached. Place the composite material at room temperature to allow the cyclohexane on the gold film surface to evaporate naturally, and you can get Au@TiO 2 Jans Structural Composites.

[0067] The same raw materials, operation process and preparation method as in Example 1 were adopted, and only the amount of trisodium citrate in S1 was changed from 3 ml to 1 ml, and the size of the prepared Au NPs became 45 nm, so it is not described in detail here. The test method was the same as that in Example 1, and the final test results were the same.

[0068] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

[0069] The final product Au@H-TiO prepared in Example 1 2 The Janus structure SERS substrate was tested as follows: Figure 1-6 shown.

[0070] Figure 1 This is a scanning electron microscope image of 16nm Au NPs. It can be seen from the figure that the gold nanoparticles have regular shapes and uniform sizes.

[0071] Figure 2 This is a scanning electron microscope image of hollow titanium dioxide. From the image, we can see that titanium dioxide has a spherical structure and its surface is covered with small holes.

[0072] Figure 3 This is a projection electron microscope image of hollow titanium dioxide. It can be seen from the image that titanium dioxide has a hollow structure, which provides the possibility for the adsorption of pollutants.

[0073] Figure 4 Au@H-TiO 2Scanning electron microscopy of the Janus structure, showing the Au NPs and H-TiO 2 Good combination, and H-TiO 2 Half of the surface is modified with Au NPs, and the other half is not modified with Au NPs, forming a Janus structure.

[0074] Figure 5 R6G in Au@H-TiO 2 Spectrum of Raman intensity changing with time on Janus structure SERS substrate.

[0075] Figure 6 R6G in Au@H-TiO 2 Raman spectra of 15 random points on the Janus structure SERS substrate.

[0076] It should be understood that the above description is for illustration and not for limitation. Many embodiments and many applications beyond the examples provided will be apparent to those skilled in the art upon reading the above description. Therefore, the scope of the present invention should not be determined with reference to the above description, but rather with reference to the appended claims and the full range of equivalents to which such claims are entitled. For the purpose of comprehensiveness, all articles and references, including disclosures of patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the preceding claims is not intended to be a waiver of the subject matter, nor should it be considered that the inventors did not consider the subject matter to be part of the disclosed inventive subject matter.

Claims

1. A method for preparing an Au@H-TiO2 Janus structure SERS substrate, characterized in that: The preparation method of the Au@H-TiO2 Janus structure SERS substrate comprises the following steps: Step S1: Preparation of gold nanoparticles Au NPs Dissolve HAuCl4·3H2O with a mass ratio of 0.5%-1.5% in deionized water to obtain a solution, wherein the volume ratio of HAuCl4·3H2O to deionized water is 0.15-1.5:90-110, heat the solution to boiling, then dropwise add sodium citrate with a mass ratio of 0.5%-1.5%, wherein the volume ratio of HAuCl4·3H2O to sodium citrate is 0.15-1.5:2-3, stop heating when the solution turns wine red, and obtain gold nanoparticles Au NPs for later use; Step S2: Preparation of hollow titanium dioxide H-TiO2 Anhydrous ethanol, polyvinyl pyrrolidone aqueous solution, hydrochloric acid and titanium tetrafluoride aqueous solution in a volume ratio of 25-30: 3-5: 0.2-0.3: 2-3 were mixed evenly and placed in a polytetrafluoroethylene liner. After standing for one hour, the suspension was heated in a reactor at 160-200°C for 3 hours. Finally, the product was centrifuged and washed with water for 3 times and dried to obtain titanium dioxide H-TiO2 with a hollow structure. Step S3: Preparation of Au@H-TiO2 Janus structure SERS substrate First, the silicon wafer needs to be modified. The silicon wafer is cut into equal-sized squares and cleaned with ethanol and deionized water. Then, the cleaned silicon wafer is placed in a boiling piranha solution for 20-40 minutes. After being taken out, it is ultrasonically cleaned six times with deionized water, each time for 15 minutes. Take 1-3 mg of the hollow titanium dioxide H-TiO2 in step S2, ultrasonically disperse it in 10-14 ml of anhydrous ethanol, drop it on the modified silicon wafer, place it at room temperature, and wait for the anhydrous ethanol on the surface to evaporate to obtain a hollow titanium dioxide film; Take 5-7mL of gold nanoparticles Au NPs in step S1, drop 1-2mL of cyclohexane to form a water / cyclohexane immiscible interface between the two phases, add anhydrous ethanol dropwise until a golden mirror reflection appears, immerse the silicon wafer carrying the hollow titanium dioxide film in the nanoparticle monolayer film, slowly withdraw the silicon wafer after it is completely attached to the gold film on the interface, and after the cyclohexane evaporates naturally at room temperature, pass protective gas into the silicon wafer carrying Au@H-TiO2 in a tubular furnace and calcine at 400-500°C for 1-3h to obtain a mixture for calcination, and peel the product from the silicon wafer substrate to obtain an Au@H-TiO2 Janus structure nanocomposite material.

2. The method for preparing a Au@H-TiO2 Janus structure SERS substrate according to claim 1, characterized in that: In the step S1, 1 ml of HAuCl4·3H2O with a mass ratio of 1% is taken, the amount of the above HAuCl4·3H2O deionized water solvent used is 100 ml, and 3 ml of sodium citrate with a mass ratio of 1% is added.

3. The method for preparing a Au@H-TiO2 Janus structure SERS substrate according to claim 1, characterized in that: In the step S2, the amount of anhydrous ethanol used is 27.6 ml, the amount of polyvinyl pyrrolidone aqueous solution used is 4 ml, the amount of hydrochloric acid used is 0.25 ml, and the amount of titanium tetrafluoride used is 2.5 ml.

4. The method for preparing a Au@H-TiO2 Janus structure SERS substrate according to claim 3, characterized in that: The concentration of the polyvinyl pyrrolidone aqueous solution is 9.75 mg / mL, the concentration of the hydrochloric acid is 0.1 M, and the concentration of the titanium tetrafluoride aqueous solution is 0.04 M.

5. The method for preparing a Au@H-TiO2 Janus structure SERS substrate according to claim 1, characterized in that: In step S3, the size of the silicon wafer is 1×1 cm; the piranha solution is prepared from concentrated sulfuric acid and 30% hydrogen peroxide by mass, the volume ratio of concentrated sulfuric acid to hydrogen peroxide is 7:3, and the silicon wafer is boiled in the piranha solution for 30 minutes.

6. The method for preparing a Au@H-TiO2 Janus structure SERS substrate according to claim 1, characterized in that: In the step S3, the amount of hollow titanium dioxide used is 2 mg, the concentration of hollow titanium dioxide is 0.003M-0.004M, the amount of anhydrous ethanol used is 12 ml, the ultrasonic time is 10 min, and the amount added to each silicon wafer is 200 μL.

7. The method for preparing a Au@H-TiO2 Janus structure SERS substrate according to claim 1, characterized in that: In step S3, the amount of gold nanoparticles Au NPs used is 6 ml, and the amount of cyclohexane used is 1.5 ml. When golden mirror reflection appears at the water / cyclohexane immiscible interface, the dropwise addition of anhydrous ethanol is stopped.

8. The method for preparing a Au@H-TiO2 Janus structure SERS substrate according to claim 1, characterized in that: In the step S3, the silicon wafer loaded with Au@H-TiO2 is calcined at a temperature of 500°C in a tube furnace for 2 hours, and N2 / H2=90 / 10 is continuously introduced as a protective gas during the calcination process.

9. An Au@H-TiO2 Janus structure SERS substrate, prepared by the method for preparing an Au@H-TiO2 Janus structure SERS substrate according to any one of claims 1 to 8, characterized in that: The Au@H-TiO2 Janus structure SERS substrate was prepared.