Pixel pattern manufacturing method, color filter and manufacturing method thereof, and liquid crystal display device
By using ultraviolet light emitting diodes with peak wavelengths of no less than 300nm and specific formula photosensitive resin compositions, the problems of poor deep curability of the photopolymerization initiator and cured film are solved, and the coating formation with excellent gradient angles is achieved and high efficiency and energy saving is achieved production method.
Patent Information
- Application Number
- CN202410570152.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, when using ultraviolet light sources, the photopolymerization initiator is prone to sublimation, resulting in pattern shape defects and reduced production efficiency. In addition, the traditional high-pressure mercury lamp has a short life and high cost, and insufficient light energy irradiated by ultraviolet LEDs leads to poor deep curability of the cured film.
UV light emitting diodes with a peak wavelength of no less than 300nm are used as exposure light sources, and combined with the photosensitive resin composition of a specific formula, including pigments, alkali-soluble resins, ethylene-containing unsaturated compounds and light-starting agents, are formed by spin coating. The film was exposed at an illumination of 50 mW/cm2 to 95 mW/cm2, followed by development and post-baking treatment.
Effectively inhibit the sublimation of the photopolymerization initiator, maintain high curability on the surface and depth of the coating film, extend the service life of the ultraviolet light-emitting diode, improve production efficiency and reduce energy consumption.
Smart Images

Figure BDA0004830596650000141 
Figure BDA0004830596650000142 
Figure BDA0004830596650000143
Abstract
Description
Technical Field
[0001] The invention provides a photosensitive resin composition with good gradient angle, and a method for manufacturing a pixel pattern and a color filter thereof. Background Art
[0002] The conventional method for producing a cured film having a fine pattern such as an interlayer insulating film, a protective film, a spacer or a color filter is to apply a photosensitive resin composition dispersed with a pigment on a substrate to form a coating film, and then irradiate (expose) the coating film with radiation using a photomask, and then obtain a cured film by development.
[0003] However, in the above-mentioned exposure process, when a conventional high-pressure mercury lamp or a metal halide lamp is used as a UV light source, the photopolymerization initiator contained in the photosensitive resin composition will be sublimated, and these sublimates will adhere to the photomask, resulting in a defect that the expected pattern shape cannot be formed. In addition, when the sublimates adhere to the photomask, the production line of the cured film must be temporarily stopped to facilitate cleaning of the mask, which will reduce production efficiency.
[0004] During the exposure process, the sublimation of the photopolymerization initiator is due to the fact that when using the conventional ultraviolet light source, the light source will emit infrared light and ultraviolet light, wherein the infrared light provides heat to the photopolymerization initiator, thus causing the sublimation of the photopolymerization initiator.
[0005] In order to avoid the above-mentioned sublimation defect of the photopolymerization initiator, Japanese Patent JP 2008-224964 has disclosed a solution, but it still cannot effectively suppress the sublimation defect of the photopolymerization initiator. In addition, the conventional high-pressure mercury lamp has a short life and needs to be replaced frequently, so its cost is also poor.
[0006] Secondly, another conventional method discloses a UV curable resin composition (see International Publication Patent WO2010 / 071171 and Japanese Patent JP 2010-126542), which uses an ultraviolet light emitting diode that does not emit infrared light as a light source. However, when using this ultraviolet LED as an exposure light source, due to the low energy of the irradiated light, even if the surface curing property of the cured film is good, the curing property in the deep part of the film is still poor.
[0007] In view of this, a method for forming a cured film is desired, which can suppress the sublimation of a photopolymerization initiator and maintain the curability of the surface and deep part of the cured film even when using an ultraviolet light curing device using an ultraviolet light emitting diode, that is, form a cured film with an excellent gradient angle. Furthermore, since the ultraviolet light emitting diode used only needs to be lit when exposure is desired, compared with the energy loss of the traditional high-pressure mercury lamp or metal halide lamp that needs to be continuously lit, the ultraviolet light emitting diode used in the method for forming a cured film has a better service life and can provide better energy-saving performance. Summary of the invention
[0008] In view of this, one aspect of the present invention is to provide a method for producing a pixel pattern, which uses a photosensitive resin composition with a good gradient angle to form a coating film, and then forms a pixel pattern by exposure. The photosensitive resin composition includes a pigment (A), an alkali-soluble resin (B), a compound containing an ethylenically unsaturated group (C), a photoinitiator (D), and a solvent (E).
[0009] Another aspect of the present invention is to provide a method for manufacturing a color filter, which utilizes the above-mentioned photosensitive resin composition to form a pixel pattern layer.
[0010] Another aspect of the present invention is to provide a color filter, which is formed by using the aforementioned manufacturing method.
[0011] Another aspect of the present invention is to provide a liquid crystal display device, which includes the aforementioned color filter.
[0012] According to the above aspect of the present invention, a method for producing a pixel pattern is provided, wherein a photosensitive resin composition is used to form a coating film on a substrate, and the coating film is subjected to an exposure process. The exposure process utilizes an ultraviolet light emitting diode to irradiate the coating film, the peak wavelength of the ultraviolet light emitting diode is not less than 300nm, and the illumination of the exposure process is 50mW / cm 2 Up to 95mW / cm 2 The photosensitive resin composition comprises a pigment (A), an alkali-soluble resin (B), a compound containing an ethylenically unsaturated group (C), a photoinitiator (D) and a solvent (E).
[0013] Method for making pixel pattern
[0014] First, prepare substrate.Substrate can use transparent glass substrates such as borosilicate glass, boroaluminosilicate glass, alkali-free glass, quartz glass, synthetic quartz glass, soda glass or pure corundum (white sapphire).And, also can use transparent resin films such as acrylic acid, polyamide, polyacetal, polybutylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, triacetyl cellulose, syndiotactic polystyrene, polyphenylene sulfide, polyether ketone, polyether ether ketone, fluororesin, polyether nitrile, polycarbonate, modified polyphenylene ether, polycyclohexene, polynorbornene resin, polysulfone, polyether sulfone, polyarylate, polyamide-imide, polyetherimide or thermoplastic polyimide of polymethyl methacrylate etc.In particular, because alkali-free glass is a material with little thermal expansion coefficient, and dimensional stability and high temperature heat treatment characteristics are excellent, it is preferred to use alkali-free glass.
[0015] According to the requirements, the substrate may be pre-treated by forming a silicon dioxide film by an appropriate method such as ion plating, sputtering, gas phase reaction or vacuum evaporation in addition to being treated with chemicals such as silane coupling agents or plasma.
[0016] Next, a light-shielding layer (black matrix) is formed on the substrate to separate the parts that form pixels. For example, a metal (chromium metal) film formed by sputtering or vapor deposition is processed into a desired pattern using a photoetching method. Alternatively, a photosensitive composition containing a black colorant is coated on the substrate, and a photoetching method is used to form the desired pattern. The film thickness of the light-shielding layer composed of the metal film is generally preferably 0.1μm to 0.2μm. Secondly, the film thickness of the light-shielding film formed using the black photosensitive composition is preferably about 1μm. In addition, there are also situations where a light-shielding layer is not required, and in this case, the step of forming the light-shielding layer can be omitted.
[0017] Then, a colored photosensitive composition is coated on the substrate, and then pre-baked to evaporate the solvent and form a coating film.
[0018] When the colored photosensitive composition is applied to the substrate, spray coating, roll coating, spin coating (spin coating), slot-die coating, or rod coating can be appropriately selected. From the viewpoint of obtaining a coating having a uniform film thickness, spin coating or slot-die coating is preferably used.
[0019] Pre-baking is usually carried out in combination with reduced pressure drying and heating drying. Reduced pressure drying is generally carried out at a pressure as low as 50Pa to 200Pa. The heating drying conditions are generally carried out at a temperature of 70°C to 110°C using a hot plate for about 1 minute to 10 minutes. The thickness of the applied coating film is generally 0.6μm to 8.0μm as the film thickness after drying, and preferably 1.2μm to 5.0μm.
[0020] In addition, other examples of forming a coating film of a colored photosensitive composition on a substrate include methods using an inkjet method as disclosed in Japanese Patent Publication No. 7-318723 and / or Japanese Patent Publication No. 2000-310706. In this method, a barrier layer having a light shielding function is first formed on the surface of the substrate. Then, a colored photosensitive composition is sprayed into the barrier layer, for example, by an inkjet device. Then, a pre-bake is performed to evaporate the solvent. The method and conditions of the pre-bake are the same as those in the above-mentioned embodiment.
[0021] The aforementioned interlayer not only has a light-shielding function, but also has the effect of preventing the various colored photosensitive compositions sprayed into the divided areas from mixing. Therefore, compared with the light-shielding layer (black matrix) used in the aforementioned embodiment, the film thickness of the interlayer is thicker. The interlayer is generally formed using a black photosensitive composition. In addition, other embodiments of forming a coating of a colored photosensitive composition on a substrate can also be listed, such as: the dry film method disclosed in Japanese Patent Publication No. JP Hei 9-5991. In this method, a colored photosensitive composition is coated on a thin film support and pre-baked to evaporate the solvent to form a dry film containing the colored photosensitive composition on the support. Then, a laminator is used to layer the support volume with a colored photosensitive composition layer on a substrate for forming a color filter. Next, the colored photosensitive composition layer is peeled off from the support to transfer the colored photosensitive composition layer to the substrate. The method of coating the colored photosensitive composition on the support, the method of pre-baking and the conditions may be the same as those in the aforementioned embodiment.
[0022] Exposure process
[0023] After the aforementioned step of forming the coating film, at least a portion of the formed coating film is exposed through a photomask having a prescribed pattern. The present invention is characterized in that the exposure light source utilized is an ultraviolet light emitting diode. An ultraviolet light emitting diode is a light emitting diode that emits ultraviolet light. For the ultraviolet light emitting diode that can be used, there is no particular limitation if the ultraviolet light emitted can be photosensitized by the photopolymerization initiator described later. However, in order to obtain a color filter with excellent chromaticity characteristics, an ultraviolet light emitting diode with a peak wavelength of more than 300nm is preferred, especially an ultraviolet light emitting diode with a peak wavelength in the range of 350nm to 400nm. In the present invention, by using an ultraviolet light emitting diode having the aforementioned luminescent characteristics as an exposure light source, the decomposition of the dye during the exposure step can be suppressed. The "peak wavelength" mentioned above refers to the wavelength at the maximum luminous intensity in the luminescent spectrum, and it can be measured using a commercially available spectrophotometer.
[0024] The exposure amount in the pixel pattern forming method of the present invention is generally 10 J / m 2 Up to 10,000 J / m 2 , and the illumination of the exposure process can be 50mW / cm 2 Up to 95mW / cm 2 , preferably 52mW / cm 2 Up to 88mW / cm 2 When the illumination of the exposure process is not within the aforementioned range, the formed pixel pattern has a poor gradient angle. The UV LED irradiation device may be a product sold by International Electrotechnical Corporation, for example.
[0025] After the exposure process, the following steps may be performed as needed: a step of developing the exposed coating film (hereinafter also referred to as “development process”); and / or a step of post-baking the coating film.
[0026] Development process
[0027] After the development process, the coating is developed with a developer to dissolve and remove the unexposed portion of the coating. The developer is preferably an alkaline developer, such as an aqueous solution of sodium carbonate, sodium hydroxide, potassium hydroxide, tetramethylammonium hydroxide, choline, 1,8-diazabicyclo[5.4.0]-7-undecene, 1,5-diazabicyclo[4.3.0]-5-nonane, etc. A water-soluble organic solvent such as methanol or ethanol, or a surfactant, etc. may also be added to the alkaline developer in an appropriate amount. Secondly, after the alkaline development treatment, water washing is generally performed.
[0028] The developing method may be, for example, a shower developing method, a spray developing method, a dipping developing method, or a puddle developing method. The developing conditions may be, for example, 5 seconds to 300 seconds at room temperature. In addition, when the coating film of the colored photosensitive composition is formed by the aforementioned inkjet method, the developing step is not required and can be omitted.
[0029] Post-baking steps for coating films
[0030] After the development process, or after the coating is formed by the inkjet method and the exposure process is performed, it is preferred to post-bake the patterned coating from the viewpoint of improving the curability. When a hot air heating furnace is used, the post-bake conditions can be set, for example, at 150° C. to 250° C. for about 20 minutes to 40 minutes.
[0031] Through the above operations, a pixel pattern and a pixel array arranged in a predetermined configuration can be formed. In detail, by repeatedly performing the above steps on the same substrate with a photosensitive composition containing a red colorant, a green colorant or a blue colorant, a color filter having a pixel pattern of the three primary colors of red, green and blue and arranged in a predetermined configuration can be obtained. However, in the embodiment of the present invention, the order of forming the pixel pattern of each color on the substrate is not limited to the above-mentioned exemplary order. The order of forming the pixel pattern of each color can be appropriately changed.
[0032] The film thickness of the pixel pattern formed by the above operation is generally 0.5 μm to 5.0 μm, and preferably 1.0 μm to 3.0 μm.
[0033] In addition, in the present invention, the pixel pattern constituting the color filter is not limited to red, green and blue, and it can also be a pixel pattern using yellow, magenta and cyan as the three primary colors. Secondly, in addition to the coloring pattern corresponding to the pixels of the three primary colors, a coloring pattern of a fourth or fifth color can also be formed. For example, the content disclosed in the Japanese Patent Publication No. JP 2005-523465, in addition to the coloring pattern corresponding to the pixels of the three primary colors such as red, green and blue, a fourth pixel (yellow pixel) or a fifth pixel (cyan pixel) for expanding the color expression range can be configured.
[0034] In the pixel pattern formed by the above operation, a protective film is further provided to improve the display characteristics of the display element. The protective film can be an organic film or an organic-inorganic hybrid film formed of a curable composition, or a SiN x Film and SiO x In the embodiment of the present case, it is preferred to use a curable composition to form the protective film.
[0035] As a method of forming a protective film using a curable resin composition, for example, the method disclosed in Japanese Laid-Open Patent Publication No. 4-53879 or Japanese Laid-Open Patent Publication No. 6-192389 can be adopted.
[0036] The curable resin composition used to form the protective film may be, for example, a thermosetting resin composition disclosed in Japanese Patent Publication No. 3-188153 or Japanese Patent Publication No. 4-53879; a photosensitive resin composition disclosed in Japanese Patent Publication No. 6-192389 or Japanese Patent Publication No. 8-183819; or a curable composition containing polyorganosiloxane disclosed in Japanese Patent Publication No. 2006-195420 or Japanese Patent Publication No. 2008-208342.
[0037] According to the method for forming a pixel pattern of the present invention, the excellent chromaticity characteristics of dyes and lake pigments can be expressed without loss, in other words, a color filter having high color purity and high brightness stimulation value (Y) in the CIE color system can be obtained. Therefore, by using the method for forming a pixel pattern of the present invention, a color filter having excellent chromaticity characteristics can be obtained. The method for forming a pixel pattern of the present invention can be used, for example, to prepare various color filters such as color filters for color liquid crystal display devices, color filters for color decomposition of solid-state imaging devices, color filters for organic electroluminescent display devices, or color filters for electronic paper, and is particularly suitable for preparing color filters used in color liquid crystal display devices using large substrates.
[0038] Pigment (A)
[0039] The pigment (A) of the present invention may be an inorganic pigment, an organic pigment or a combination thereof.
[0040] The inorganic pigment can be a metal compound such as a metal oxide or a metal salt, which can be selected from oxides of metals such as iron, cobalt, aluminum, cadmium, lead, copper, titanium, magnesium, chromium, lead, antimony, composite oxides of the aforementioned metals, and metal salts.
[0041] The organic pigment can be selected from CI Pigment Yellow 1, 3, 11, 12, 13, 14, 15, 16, 17, 20, 24, 31, 53, 55, 60, 61, 65, 71, 73, 74, 81, 83, 93, 95, 97, 98, 99, 100, 101, 104, 106, 108, 109, 110, 113, 114, 116, 117, 119, 120, 126, 127, 128, 129, 138, 139, 150, 151, 152, 153, 154, 155, 156, 166, 167, 1 68, 175; CI Pigment Orange 1, 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 61, 63, 64, 71, 73; CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 50:1, 52:1, 53:1, 57, 57:1, 57:2, 58:2, 58:4, 60:1, 63:1, 63:2, 64:1, 81:1, 83, 88, 90:1, 97, 101, 102, 104, 105, 106, 108, 112, 113, 114, 122, 123, 144, 146, 149, 150, 151, 155, 166, 168, 170, 171, 172, 174, 175, 176, 177, 178, 179, 180, 185, 187, 188, 190, 193, 194, 202, 206, 207, 208, 209, 215, 216, 220, 224, 226, 242, 243, 245, 254, 255, 264, 265; CI Pigment Violet 1, 14, 19, 23, 29, 32, 33, 36, 37, 38, 39, 40, 50; CI Pigment Blue 1, 2, 15, 15:1, 15:2, 15:3, 15:4, 15:5, 15:6, 16, 21, 22, 60, 61, 64, 66; CI Pigment Green 7, 36, 37, 42, 58; CI Pigment Brown 23, 25, 28; and CI Pigment Black 1, 7. The above organic pigments may be used alone or in combination.
[0042] The average particle size of the pigment (A) is preferably 10 nm to 200 nm, more preferably 20 nm to 150 nm, and particularly preferably 30 nm to 130 nm.
[0043] Based on 100 parts by weight of the total amount of the alkali-soluble resin (B), the amount of the pigment (A) is 5 to 300 parts by weight, preferably 10 to 250 parts by weight, and more preferably 15 to 200 parts by weight.
[0044] If necessary, the pigment (A) may also selectively use a dispersant, for example, a cationic, anionic, nonionic, amphoteric, polysiloxane or fluorine-based surfactant.
[0045] The aforementioned surfactants may include but are not limited to polyethylene oxide alkyl ethers such as polyethylene oxide dodecyl ether, polyethylene oxide stearyl ether, and polyethylene oxide oleyl ether; polyethylene oxide alkyl phenyl ether surfactants such as polyethylene oxide octyl phenyl ether and polyethylene oxide nonyl phenyl ether; polyethylene glycol diester surfactants such as polyethylene glycol dilaurate and polyethylene glycol distearate; sorbitan fatty acid ester surfactants; fatty acid-modified polyester surfactants; tertiary amine-modified polyurethane surfactants; Shin-Etsu Chemical Co., Ltd., product model KP; Toray Dow Corning Silicon Co., Ltd., product model SF-8427; Kyoeisha Oil Chemical Co., Ltd., product model Polyflow; Tochem Products Co., Ltd.) with the model number F-Top; Dainippon Ink Chemical Co., Ltd. with the model number Megafac; Sumitomo 3M with the model number Fluorad; Asahi Glass with the model numbers Asahi Guard and Surflon. The aforementioned surfactants may be used alone or in combination.
[0046] Alkali soluble resin (B)
[0047] The alkali-soluble resin (B) of the present invention is obtained by reacting an ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides, an ethylenically unsaturated monomer (B-2) having an epoxy group, and other copolymerizable ethylenically unsaturated monomers (B-3).
[0048] In the aforementioned ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides, the ethylenically unsaturated monomer having one or more carboxylic acids may include but is not limited to an unsaturated monocarboxylic acid compound, an unsaturated polycarboxylic acid compound, a polycyclic compound having an unsaturated group and one carboxylic acid group, or a polycyclic compound having an unsaturated group and multiple carboxylic acid groups.
[0049] The unsaturated monocarboxylic acid compound may include but is not limited to (meth) acrylic acid, crotonic acid, α-chloroacrylic acid, ethyl acrylic acid, cinnamic acid, 2-(meth)acryloyloxy ethylsuccinate monoester, 2-(meth)acryloyloxy ethylsuccinate monoester, 2-(meth)acryloyloxy ethylsuccinate hexahydrophthalate, 2-(meth)acryloyloxy ethylsuccinate phthalate or omega-carboxylic acid-based polycaprolactone polyol monoacrylate, etc. The omega-carboxylic acid-based polycaprolactone polyol monoacrylate may be a product manufactured by East Asia Synthetics and is modeled as ARONIX M-5300.
[0050] The unsaturated polycarboxylic acid compound may include but is not limited to maleic acid, fumaric acid, methyl fumaric acid, itaconic acid or citraconic acid.
[0051] The aforementioned polycyclic compound having an unsaturated group and one carboxylic acid group may include, but is not limited to, 5-carboxylic acid bicyclo[2.2.1]hept-2-ene, 5-carboxylic acid-5-methylbicyclo[2.2.1]hept-2-ene, 5-carboxylic acid-5-ethylbicyclo[2.2.1]hept-2-ene, 5-carboxylic acid-6-methylbicyclo[2.2.1]hept-2-ene or 5-carboxylic acid-6-ethylbicyclo[2.2.1]hept-2-ene.
[0052] The polycyclic compound having an unsaturated group and a plurality of carboxylic acid groups may include 5,6-dicarboxylic acid bicyclo[2.2.1]hept-2-ene and the like.
[0053] Preferably, the ethylenically unsaturated monomer having one or more carboxylic acids is selected from acrylic acid, methacrylic acid, 2-methacryloylethoxysuccinate, 2-methacryloylethoxyhexahydrophthalate, or any combination thereof.
[0054] In the aforementioned ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides, the ethylenically unsaturated monomer having one or more carboxylic anhydrides may include but is not limited to unsaturated carboxylic anhydride compounds or polycyclic compounds having an unsaturated group and a carboxylic anhydride.
[0055] The unsaturated carboxylic anhydride compound may include but is not limited to maleic anhydride, fumaric anhydride, methylfumaric anhydride, itaconic anhydride or citraconic anhydride, etc. The polycyclic compound having an unsaturated group and a carboxylic anhydride may include but is not limited to 5,6-dicarboxylic anhydride bicyclo[2.2.1]hept-2-ene, etc.
[0056] Preferably, the ethylenically unsaturated monomer having one or more carboxylic anhydrides is maleic anhydride.
[0057] The ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides may be used alone or in combination of two or more.
[0058] In a specific example of the present invention, based on the total usage of 100 parts by weight of copolymerizable monomers such as the ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides, the ethylenically unsaturated monomer (B-2) having an epoxy group, and the other copolymerizable ethylenically unsaturated monomers (B-3), the usage of the ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides is 10 to 60 parts by weight, preferably 15 to 55 parts by weight, and more preferably 20 to 50 parts by weight.
[0059] The ethylenically unsaturated monomer (B-2) having an epoxy group may include, but is not limited to, a (meth)acrylate compound having an epoxy group, an α-alkylacrylate compound or a glycidyl ether compound having an epoxy group.
[0060] The aforementioned (meth)acrylate compound having an epoxy group may include but is not limited to glycidyl (meth)acrylate, 2-methylglycidyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 6,7-epoxyheptyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate or 3,4-epoxycyclohexylmethyl (meth)acrylate, etc.
[0061] The aforementioned α-alkyl acrylate compound having an epoxy group may include, but is not limited to, α-ethyl acrylate glycidyl ester, α-n-propyl acrylate glycidyl ester, α-n-butyl acrylate glycidyl ester, α-ethyl acrylate-6,7-epoxyheptyl ester, and the like.
[0062] The aforementioned glycidyl ether compound may include but is not limited to o-vinylbenzylglycidyl ether (o-vinylbenzylglycidyl ether), m-vinylbenzylglycidyl ether (m-vinylbenzylglycidyl ether) or p-vinylbenzylglycidyl ether (p-vinylbenzylglycidyl ether) and the like.
[0063] The ethylenically unsaturated monomer (B-2) having an epoxy group may be used alone or in combination of two or more.
[0064] Preferably, the aforementioned ethylenically unsaturated monomer having an epoxy group (B-2) is selected from glycidyl methacrylate, 2-methylglycidyl methacrylate, 3,4-epoxycyclohexylmethyl methacrylate, 6,7-epoxyheptyl methacrylate, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether or any combination thereof.
[0065] In a specific example of the present invention, based on the total usage of the copolymerizable monomers such as the ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides, the ethylenically unsaturated monomer (B-2) having an epoxy group, and the other copolymerizable ethylenically unsaturated monomers (B-3) is 100 parts by weight, the usage of the ethylenically unsaturated monomer (B-2) having an epoxy group is 1 to 50 parts by weight, preferably 3 to 45 parts by weight, and more preferably 5 to 40 parts by weight.
[0066] The aforementioned other copolymerizable ethylenically unsaturated monomers (B-3) may include, but are not limited to, alkyl (meth)acrylates, alicyclic (meth)acrylates, aryl (meth)acrylates, unsaturated dicarboxylates, hydroxyalkyl (meth)acrylates, polyethers having a (meth)acrylate group, styrene compounds, or unsaturated compounds other than the above compounds.
[0067] The above-mentioned alkyl (meth)acrylate may include but is not limited to methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate or t-butyl (meth)acrylate, etc.
[0068] The above-mentioned alicyclic (meth)acrylates may include but are not limited to cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, dicyclopentyl (meth)acrylate (or tricyclo[5.2.1.0 2,6 ]dec-8-yl (meth)acrylate), dicyclopentyloxyethyl (meth)acrylate, isobornyl (meth)acrylate or tetrahydrofuran (meth)acrylate, etc.
[0069] The aryl (meth)acrylate may include but is not limited to phenyl (meth)acrylate or benzyl methacrylate.
[0070] The unsaturated dicarboxylic acid esters may include but are not limited to diethyl maleate, diethyl fumarate or diethyl itaconate.
[0071] The aforementioned hydroxyalkyl (meth)acrylate may include but is not limited to 2-hydroxyethyl (meth)acrylate or 2-hydroxypropyl (meth)acrylate.
[0072] The aforementioned polyether having a (meth)acrylate group may include but is not limited to polyethylene glycol mono(meth)acrylate or polypropylene glycol mono(meth)acrylate.
[0073] The aforementioned styrene-based compounds may include but are not limited to styrene, α-methylstyrene, m-methylstyrene, p-methylstyrene or p-methoxystyrene.
[0074] Unsaturated compounds other than the above compounds may include, but are not limited to, acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, acrylamide, methacrylamide, vinyl acetate, 1,3-butadiene, isoprene, 2,3-dimethyl 1,3-butadiene, N-succinimidyl-3-maleimidobenzoate, N-succinimidyl-4-maleimidobutyrate, N-succinimidyl-6-maleimidohexanoate, N-succinimidyl-3-maleimidopropionate, N-(9-acridinyl)maleimide, N-octylmaleimide, N-cyclohexylmaleimide, or N-phenylmaleimide.
[0075] The above-mentioned other copolymerizable ethylenically unsaturated monomers (B-3) may be used alone or in combination of two or more.
[0076] Preferably, the aforementioned other copolymerizable ethylenically unsaturated monomers (B-3) are selected from methyl (meth)acrylate, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, tert-butyl (meth)acrylate, benzyl (meth)acrylate, dicyclopentyl (meth)acrylate, isobornyl methacrylate, dicyclopentyloxyethyl (meth)acrylate, styrene, p-methoxystyrene or any combination of the above compounds.
[0077] In a specific example of the present invention, the total amount of copolymerizable monomers such as the ethylenically unsaturated monomer (B-1) having one or more carboxylic acids or carboxylic anhydrides, the ethylenically unsaturated monomer (B-2) having an epoxy group and the other copolymerizable ethylenically unsaturated monomer (B-3) is 100 parts by weight, and the amount of the other copolymerizable ethylenically unsaturated monomer (B-3) is 10 to 90 parts by weight, preferably 15 to 85 parts by weight, and more preferably 20 to 80 parts by weight.
[0078] When preparing the alkali-soluble resin (B), a solvent may be used. The solvent may be used alone or in combination. The solvent includes but is not limited to (poly)alkylene glycol monoalkyl ethers such as ethylene glycol methyl ether, ethylene glycol ethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol n-propyl ether, diethylene glycol n-butyl ether, triethylene glycol methyl ether, triethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol n-propyl ether, dipropylene glycol n-butyl ether, tripropylene glycol methyl ether, tripropylene glycol ethyl ether; ethylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, propylene glycol methyl ether acetate; acetate; PGMEA), propylene glycol ethyl ether acetate and other (poly) alkylene glycol monoalkyl ether acetates; other ethers such as diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, tetrahydrofuran, etc.; ketones such as methyl ethyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, etc.; alkyl lactates such as methyl 2-hydroxypropionate and ethyl 2-hydroxypropionate; methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate (ethyl 3-ethoxypropionate; EEP), ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-methoxybutyrate and other esters; aromatic hydrocarbons such as toluene and xylene; amides such as nitrogen-methylpyrrolidone (NMP), nitrogen, nitrogen-dimethylformamide (DMF), or nitrogen, nitrogen-dimethylacetamide (DMAC), etc. Preferably, the solvent is selected from propylene glycol methyl ether acetate, ethyl 3-ethoxypropionate, or a combination thereof. The (poly)alkylene glycol monoalkyl ethers refer to alkylene glycol monoalkyl ethers or polyalkylene glycol monoalkyl ethers. The (poly)alkylene glycol monoalkyl ether acetates refer to alkylene glycol monoalkyl ether acetates or polyalkylene glycol monoalkyl ether acetates.
[0079] The initiator used in the preparation of the alkali-soluble resin (B) is generally a free radical polymerization initiator, for example: azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis-2-methylbutyronitrile (2,2'-azobis-2-methyl butyronitrile; AMBN); and peroxide compounds such as dibenzoyl peroxide.
[0080] The alkali-soluble resin (B) has a polystyrene-equivalent weight average molecular weight measured by colloid permeation chromatography (GPC) of generally 1,000 to 35,000, preferably 3,000 to 30,000, and more preferably 5,000 to 25,000.
[0081] Compounds containing ethylenically unsaturated groups (C)
[0082] The ethylenically unsaturated group-containing compound (C) of the present invention may include an unsaturated compound having at least one ethylenically unsaturated group and an unsaturated compound having at least two ethylenically unsaturated groups.
[0083] Specific examples of the unsaturated compound having at least one ethylenically unsaturated group may include, but are not limited to, acrylamide, acryloyl morpholine, methacryloyl morpholine, 7-amino-3,7-dimethyloctyl acrylate, 7-amino-3,7-dimethyloctyl methacrylate, isobutoxymethylacrylamide, isobutoxymethylmethacrylamide, isobornyloxyethyl acrylate, isobornyloxyethyl methacrylate, isobornyl acrylate, isobornyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate. , ethyl diglycol acrylate, ethyl diglycol methacrylate, tert-octyl acrylamide, tert-octyl methacrylamide, diacetone acrylamide, diacetone methacrylamide, dimethylamino acrylate, dimethylamino methacrylate, dodecyl acrylate, dodecyl methacrylate, dicyclopentenyloxyethyl acrylate, dicyclopentenyloxyethyl methacrylate, dicyclopentenyl acrylate, dicyclopentenyl methacrylate, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, tetrachlorophenyl acrylate, methyl Tetrachlorophenyl acrylate, 2-tetrachlorophenoxyethyl acrylate, 2-tetrachlorophenoxyethyl methacrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, tetrabromophenyl acrylate, tetrabromophenyl methacrylate, 2-tetrabromophenoxyethyl acrylate, 2-tetrabromophenoxyethyl methacrylate, 2-trichlorophenoxyethyl acrylate, 2-trichlorophenoxyethyl methacrylate, tribromophenyl acrylate, tribromophenyl methacrylate, 2-tribromophenoxyethyl acrylate, 2-tribromophenoxyethyl methacrylate , 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, vinyl caprolactam, N-vinyl pyroxanone, phenoxyethyl acrylate, phenoxyethyl methacrylate, pentachlorophenyl acrylate, pentachlorophenyl methacrylate, pentabromophenyl acrylate, pentabromophenyl methacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, polypropylene glycol monoacrylate, polypropylene glycol monomethacrylate, bornyl acrylate, or bornyl methacrylate, etc. Among them, the unsaturated compound having at least one ethylenically unsaturated group can be used alone or in combination of multiple types.
[0084] Specific examples of the unsaturated compound having at least two ethylenically unsaturated groups include, but are not limited to, ethylene glycol diacrylate, ethylene glycol dimethacrylate, dicyclopentenyl diacrylate, dicyclopentenyl dimethacrylate, triethylene glycol diacrylate, tetraethylene glycol dimethacrylate, tris(2-hydroxyethyl)isocyanate diacrylate, tris(2-hydroxyethyl)isocyanate dimethacrylate, tris(2-hydroxyethyl)isocyanate triacrylate, tris(2-hydroxyethyl)isocyanate trimethacrylate, caprolactone-modified tris(2-hydroxyethyl)isocyanate triacrylate, caprolactone-modified tris(2-hydroxyethyl)isocyanate trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, ethylene oxide (hereinafter referred to as EO)-modified tris(2-hydroxyethyl)isocyanate triacrylate, and tris(2-hydroxyethyl)isocyanate trimethacrylate. propylene oxide (hereinafter referred to as PO) modified trimethylolpropane triacrylate, PO modified trimethylolpropane trimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, pentaerythritol tetraacrylate, pentaerythritol tetramethacrylate, polyester diacrylate, polyester dimethacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, dipentaerythritol hexaacrylate (dipentaerythritol hexaacrylate;DPHA), dipentaerythritol hexamethacrylate, dipentaerythritol pentaacrylate, dipentaerythritol pentamethacrylate, dipentaerythritol tetraacrylate, dipentaerythritol tetramethacrylate, caprolactone-modified dipentaerythritol hexaacrylate, caprolactone-modified dipentaerythritol hexamethacrylate, caprolactone-modified dipentaerythritol pentaacrylate, caprolactone-modified dipentaerythritol pentamethacrylate, tetraacrylate ditrimethylolpropane, tetramethacrylate ditrimethylolpropane, EO-modified bisphenol A diacrylate, EO-modified bisphenol A dimethacrylate, PO-modified bisphenol A diacrylate , PO modified bisphenol A dimethacrylate, EO modified hydrogenated bisphenol A diacrylate, EO modified hydrogenated bisphenol A dimethacrylate, PO modified hydrogenated bisphenol A diacrylate, PO modified hydrogenated bisphenol A dimethacrylate, PO modified glycerol tripropionate, EO modified bisphenol F diacrylate, EO modified bisphenol F dimethacrylate, phenolic polyglycidyl ether acrylate, phenolic polyglycidyl ether methacrylate, a product manufactured by Toagosei Co., Ltd. with a model number of TO-1382, or a product manufactured by Nippon Kayaku Co., Ltd. with a model number of KAYARAD DPCA-12, KAYARAD DPCA-20, KAYARAD DPCA-30, KAYARAD DPCA-60 or KAYARAD DPCA-120, etc. Among them, the unsaturated compound having at least two ethylenically unsaturated groups can be used alone or in combination of multiple types. ;
[0085] Preferably, the compound (C) containing an ethylenically unsaturated group is selected from trimethylolpropane triacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, dipentaerythritol pentaacrylate, dipentaerythritol tetraacrylate, caprolactone-modified dipentaerythritol hexaacrylate, ditrimethylolpropane tetraacrylate, PO-modified glycerol tripropionate, KAYARAD DPCA-12, KAYARAD DPCA-20, KAYARAD DPCA-30, KAYARAD DPCA-60 or KAYARAD DPCA-120 or any combination thereof.
[0086] The above-mentioned ethylenically unsaturated group-containing compound (C) may be used alone or in combination of two or more.
[0087] Based on the total usage of 100 parts by weight of the alkali-soluble resin (B), the usage of the compound (C) containing an ethylenically unsaturated group is 20 to 200 parts by weight, preferably 30 to 180 parts by weight, and more preferably 50 to 150 parts by weight.
[0088] Photoinitiator (D)
[0089] The photoinitiator (D) of the present invention may include, for example, but is not limited to, an oxime ester compound (D-1) represented by the following formula (I), an oxime ester compound (D-2) represented by the following formula (II), an oxime ester compound (D-3) represented by the following formula (III), and other photoinitiators (D-4).
[0090] Oxime ester compound (D-1) represented by formula (I)
[0091] The photoinitiator (D) may include an oxime ester compound (D-1) as shown in the following formula (I). The oxime ester compound (D-1) as shown in the formula (I) can usually generate free radicals by light irradiation, and has high sensitivity to i-rays used as a light source during patterning.
[0092]
[0093] In formula (I), Y1 represents an organic group as shown in the following formula (I-1); Y2 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; Y3 represents an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an aryl group having 6 to 10 carbon atoms.
[0094]
[0095] In formula (I-1), Y4 represents a monovalent organic group; X1 represents an oxygen atom, a sulfur atom or a carbonyl group; and a represents an integer from 0 to 5.
[0096] In formula (I), Y2 preferably represents an alkyl group having 1 to 10 carbon atoms (more preferably 1 to 8), and more preferably represents a methyl group or a hexyl group. Y3 preferably represents an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 10 carbon atoms, and more preferably represents a methyl group or a phenyl group. In formula (I-1), X1 preferably represents a sulfur atom; Y4 preferably represents a hydroxyalkoxy group having 1 to 4 carbon atoms; and a is preferably 0 or 1. Secondly, formula (I-1) may also be, for example, an organic group represented by the following formula (I'-1), wherein the definitions of X1 and Y4 are as described above and are not further described here.
[0097]
[0098] In some specific examples, the oxime ester compound (D-1) represented by formula (I) may include but is not limited to the compounds represented by the following formula (I-2) and formula (I-3).
[0099]
[0100] Based on the total usage of the alkali-soluble resin (B) being 100 parts by weight, the usage of the oxime ester compound (D-1) as shown in formula (I) can be 1 to 100 parts by weight, preferably 5 to 90 parts by weight, and more preferably 10 to 80 parts by weight.
[0101] When the photosensitive resin composition of the present invention comprises the oxime ester compound (D-1) as shown in formula (I), the formed pixel pattern has a better gradient angle.
[0102] Oxime ester compound (D-2) represented by formula (II)
[0103] The photoinitiator (D) may include an oxime ester compound (D-2) represented by the following formula (II).
[0104]
[0105] In formula (II), Z1 represents an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, a phenyl group and a tolyl group; Z2 represents an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms or a substituted or unsubstituted phenyl group; Z3 represents a substituted or unsubstituted fluorenyl group or a substituted or unsubstituted carbazolyl group.
[0106] The substituents of the aforementioned phenyl, fluorenyl and carbazolyl groups may include an alkyl group having 1 to 12 carbon atoms (preferably 1 to 4 carbon atoms), an alkoxy group having 1 to 12 carbon atoms (preferably 1 to 4 carbon atoms), a nitro group, or a benzyl group. Among them, the alkyl group and the alkoxy group may be optionally substituted by fluorine, and the benzyl group may be substituted by an alkyl group having 1 to 4 carbon atoms. In addition, the benzene ring of the fluorenyl and carbazolyl groups may be fused with another benzene ring. For example, it may be a benzocarbazolyl group.
[0107] From the viewpoint of improving photocurability, the oxime ester compound (D-2) represented by formula (II) is preferably a compound represented by the following formula (II-1).
[0108]
[0109] In formula (II-1), Z1 and Z2 are as defined above. Z4 represents an alkyl group having 1 to 6 carbon atoms, preferably an ethyl group; Z5 represents an alkyl group having 1 to 12 carbon atoms or an organic group having an acetal bond, preferably a methyl group or a substituent corresponding to Z5 in the compound shown in formula (II-1-2); b represents an integer from 1 to 3, preferably 1 or 2.
[0110] In some specific examples, the oxime ester compound (D-2) represented by the above formula (II) may include but is not limited to the compounds represented by the following formula (II-1-1) or (II-1-2), which are respectively manufactured by BASF and have the model number IRGACURE OXE-02, and manufactured by ADEKA and have the model number Optomer N-1919.
[0111]
[0112]
[0113] Preferably, the oxime ester compound (D-2) represented by formula (II) may include but is not limited to the compound represented by the following formula (II-1-3).
[0114]
[0115] Based on the total usage of the alkali-soluble resin (B) being 100 parts by weight, the usage of the oxime ester compound (D-2) represented by formula (II) is 1 to 100 parts by weight, preferably 5 to 90 parts by weight, and more preferably 10 to 80 parts by weight.
[0116] When the photosensitive resin composition of the present invention includes the oxime ester compound (D-2) represented by formula (II), the formed pixel pattern has a better gradient angle.
[0117] Oxime ester compound (D-3) represented by formula (III)
[0118] The photoinitiator (D) may include an oxime ester compound (D-3) represented by the following formula (III).
[0119]
[0120] In formula (III), R1, R2, R3, R4, R5, R6, R7 and R8 independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, COR 16 , a group represented by the following formula (III'-1);
[0121]
[0122] Or R1 and R2, R2 and R3, R3 and R4, R5 and R6, R6 and R7 or R7 and R8 independently represent a group represented by the following formula (III'-2);
[0123]
[0124] However, the condition is that at least one pair of R1 and R2, R2 and R3, R3 and R4, R5 and R6, R6 and R7 or R7 and R8 is a group represented by formula (III'-2),
[0125] R9, R 10 , R 11 and R 12 independently of one another represent a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, wherein the alkyl group having 1 to 20 carbon atoms is unsubstituted or substituted by one or more of the following groups: halogen or phenyl;
[0126] or R9, R 10 , R 11 and R 12 independently of one another represent unsubstituted phenyl or phenyl substituted by one or more of the following groups: alkyl having a carbon number of 1 to 6 or halogen;
[0127] X2 represents CO or a single bond;
[0128] R 13 represents an alkyl group having 1 to 20 carbon atoms, which is unsubstituted or substituted by one or more of the following groups: halogen, R 17 、COOR 17 OR 17 ;
[0129] or R 13 represents an alkyl group having 2 to 20 carbon atoms, which is interrupted by one or more O or CO atoms, wherein the interrupted alkyl group having 2 to 20 carbon atoms is unsubstituted or substituted by one or more halogen atoms;
[0130] or R 13 represents phenyl or naphthyl, each of which is unsubstituted or substituted with one or more of the following groups: an alkyl group having 1 to 20 carbon atoms or a haloalkyl group having 1 to 4 carbon atoms;
[0131] R 14 represents a hydrogen atom, an alkoxy group having 1 to 20 carbon atoms, or an alkyl group having 1 to 20 carbon atoms;
[0132] R 15 represents an aryl group having 6 to 20 carbon atoms, each of which is unsubstituted or substituted by one or more of the following groups: halogen, haloalkyl group having 1 to 4 carbon atoms, OR 17 , an alkyl group with a carbon number of 2 to 20 interrupted by one or more O; or each of them is substituted by an alkyl group with a carbon number of 1 to 20, and the alkyl group with a carbon number of 1 to 20 is unsubstituted or substituted by one or more of the following groups: halogen, COOR 17 , phenyl or OR 17 ;
[0133] or R 15represents a hydrogen atom, a cycloalkyl group having 3 to 8 carbon atoms; or R 15 represents an alkyl radical having 1 to 20 carbon atoms, which is unsubstituted or substituted by one or more of the following groups: halogen or a cycloalkyl radical having 3 to 8 carbon atoms;
[0134] R 16 represents an aryl group having 6 to 20 carbon atoms, each of which is unsubstituted or substituted by one or more of the following groups: halogen, haloalkyl group having 1 to 4 carbon atoms, OR 17 ; or each of them is substituted with one or more alkyl groups having a carbon number of 1 to 20, the alkyl groups having a carbon number of 1 to 20 are unsubstituted or substituted with one or more of the following groups: halogen or OR 17 ;
[0135] R 17 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, which is unsubstituted or substituted by one or more of the following groups: a halogen or a cycloalkyl group having 3 to 20 carbon atoms interrupted by one or more O atoms;
[0136] or R 17 represents an alkyl group having 2 to 20 carbon atoms, in which one or more O atoms are interspersed;
[0137] or R 17 represents phenyl, each of which is unsubstituted or substituted by one or more of the following groups: halogen, alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms;
[0138] However, the condition is that there is at least one group represented by formula (III'-1) in formula (III).
[0139] The compound of formula (III) is characterized in that it contains one or more annelated unsaturated rings on the carbazole portion. In other words, at least one pair of R1 and R2, R2 and R3, R3 and R4, R5 and R6, R6 and R7 or R7 and R8 is a group represented by formula (III'-2).
[0140] The aforementioned alkyl group with a carbon number of 1 to 20 may be a linear alkyl group or a branched alkyl group. In some specific examples, the alkyl group with a carbon number of 1 to 20 may include, but is not limited to, a methyl group, an ethyl group, a propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2,4,4-trimethylpentyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, or other appropriate alkyl groups.
[0141] The aforementioned halogenated alkyl group having 1 to 4 carbon atoms may be the aforementioned alkyl group having 1 to 4 carbon atoms substituted with halogen as defined below. The halogenated alkyl group may be, for example, monohalogenated or polyhalogenated until all hydrogen atoms are replaced with halogen. Its structure may be, for example, Cz H x Hal y , wherein x+y=2z+1, and Hal represents a halogen (preferably F). For example, the haloalkyl group having 1 to 4 carbon atoms may include but is not limited to chloromethyl, trichloromethyl, trifluoromethyl, 2-bromopropyl, or other suitable haloalkyl groups, and may preferably be trifluoromethyl or trichloromethyl.
[0142] The aforementioned alkyl group with a carbon number of 2 to 20 and interspersed with one or more O may be, for example, interspersed with O 1 to 9 times, 1 to 5 times, 1 to 3 times, 1 time or 2 times. Two interspersed O atoms may be separated by at least one methylene group, and preferably by at least two methylene groups (i.e., ethylene groups). The alkyl group is a straight chain or a branched chain. For example, the alkyl group with a carbon number of 2 to 20 and interspersed with one or more O may have the following structural units: -CH2-CH2-O-CH2CH3, -(CH2CH2O) d -CH3 (wherein d represents 1 to 9), -(CH2-CH2O)7-CH2CH3, -CH2-CH(CH3)-O-CH2-CH2CH3, or -CH2-CH(CH3)-O-CH2-CH3.
[0143] The alkoxy group having 1 to 12 carbon atoms is an alkyl group having 1 to 12 carbon atoms substituted with one O atom.
[0144] In some specific examples, the aforementioned aryl group having 6 to 20 carbon atoms may be, for example, phenyl, naphthyl, anthracenyl, phenanthrenyl, pyrenyl, The present invention relates to a phenyl group, a naphthyl group, a tetraphenyl group, a triphenyl group, or other suitable aryl groups, especially phenyl or naphthyl, and preferably phenyl. The naphthyl group may be 1-naphthyl or 2-naphthyl.
[0145] The substituted aryl groups, such as phenyl, naphthyl or aryl groups with 6 to 20 carbon atoms, may be substituted 1 to 7 times, 1 to 6 times or 1 to 4 times, respectively, in particular 1, 2 or 3 times. Obviously, the defined aryl groups cannot have more substituents than the free positions at the aryl ring.
[0146] The substituent on the phenyl ring is preferably in position 4 on the phenyl ring, or in a 3,4-, 3,4,5-, 2,6-, 2,4- or 2,4,6-bonding configuration.
[0147] A group which is interrupted once or more than once may, for example, be interrupted 1 to 19 times, 1 to 15 times, 1 to 12 times, 1 to 9 times, 1 to 7 times, 1 to 5 times, 1 to 4 times, 1 to 3 times, 1 time, or 2 times. Obviously, the number of intercalating atoms depends on the number of carbon atoms of the group to be interrupted). A substituted group which is substituted once or more than once may, for example, have 1 to 7, 1 to 5, 1 to 4, 1 to 3, 1, or 2 identical or different substituents.
[0148] The group substituted by one or more defined substituents is intended to have one substituent or multiple substituents as given, which are identical or different in definition. Halogen can be fluorine, chlorine, bromine or iodine, in particular fluorine, chlorine or bromine, and preferably fluorine or chlorine. If R1 and R2, R2 and R3, R3 and R4 or R5 and R6, R6 and R7, and R7 and R8 of formula (III) are independently of each other and are collectively a group as shown in formula (III'-2), the oxime ester compound (D-3) shown in formula (III) can, for example, have a structure as shown in the following formula (III-a) to formula (III-i).
[0149]
[0150]
[0151] Preferably, the oxime ester compound (D-3) shown in formula (III) may have a structure as shown in formula (III-a), formula (III-b) or formula (III-c), more preferably has a structure as shown in formula (III-a) or formula (III-c), or a structure as shown in formula (III-a), formula (III-c) or formula (III-d), and is particularly preferably a structure as shown in formula (III-a).
[0152] For example, R 15 It may represent a hydrogen atom, a phenyl group or a naphthyl group, wherein the phenyl group or the naphthyl group is unsubstituted or substituted with an alkyl group having 1 to 8 carbon atoms or OR 17 replaced by; or R 15 represents an alkyl group having 1 to 20 carbon atoms; or R 15 represents an alkyl group having 2 to 20 carbon atoms, wherein one or more O groups are interspersed therein.
[0153] For example, R 16 represents an aryl group having 6 to 20 carbon atoms (preferably phenyl or naphthyl, and more preferably phenyl), each of which is unsubstituted or substituted by one or more of the following groups: halogen, haloalkyl group having 1 to 4 carbon atoms, or OR 17 ; or each of them is substituted by one or more alkyl groups having 1 to 20 carbon atoms, the alkyl groups having 1 to 20 carbon atoms are unsubstituted or substituted by one or more of the following groups: halogen or OR 17 .
[0154] In addition, R 16 For example, it may represent phenyl or naphthyl, preferably phenyl or carbazole, wherein phenyl or naphthyl is unsubstituted or substituted by one or more of the following groups: halogen, haloalkyl having 1 to 4 carbon atoms, OR 17 or an alkyl group having 1 to 20 carbon atoms.
[0155] R 16 It may represent, for example, phenyl or naphthyl, preferably phenyl, each of which is unsubstituted or substituted by one or more of the following groups: halogen, OR 17 or an alkyl group having 1 to 20 carbon atoms.
[0156] Preferably, R 16 is a phenyl group, and is substituted by one or more alkyl groups having 1 to 20 carbon atoms.
[0157] R 17 For example, it may represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, wherein the alkyl group having 1 to 20 carbon atoms is unsubstituted or substituted by one or more of the following groups: a halogen or a cycloalkyl group having 3 to 20 carbon atoms interrupted by one or more O; or R 17 represents phenyl, each of which is unsubstituted or substituted by one or more of the following groups: halogen, alkyl having 1 to 12 carbon atoms or alkoxy having 1 to 12 carbon atoms.
[0158] In some specific examples, the oxime ester compound (D-3) represented by formula (III) may include but is not limited to the compounds represented by the following formulas (III-1) to (III-22).
[0159]
[0160]
[0161]
[0162]
[0163]
[0164]
[0165]
[0166]
[0167] The aforementioned oxime ester compounds (D-3) may be used alone or in combination of two or more.
[0168] Based on the total usage of the alkali-soluble resin (B) being 100 parts by weight, the usage of the oxime ester compound (D-3) represented by formula (III) can be 1 to 100 parts by weight, preferably 5 to 90 parts by weight, and more preferably 10 to 80 parts by weight.
[0169] When the photosensitive resin composition includes the oxime ester compound (D-3) represented by formula (III), the formed pixel pattern has a better gradient angle.
[0170] Other photoinitiators (D-4)
[0171] The photoinitiator (D) of the present invention may optionally contain other photoinitiators (D-4).
[0172] The other photoinitiator (D-4) can be selected from acetophenone compounds, biimidazole compounds or a combination of these compounds.
[0173] The acetophenone compound can be selected from p-dimethylamino-acetophenone, α,α'-dimethoxyazoxy-acetophenone, 2,2'-dimethyl-2-phenyl-acetophenone, p-methoxy-acetophenone, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, or 2-benzyl-2-N,N-di-methylamino-1-(4-morpholinophenyl)-1-butanone.
[0174] The above-mentioned diimidazole compound can be selected from 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-biimidazole, 2,2'-bis(o-fluorophenyl)-4,4',5,5'-tetraphenyl-biimidazole, 2,2'-bis(o-methylphenyl)-4,4',5,5'-tetraphenyl-biimidazole, 2,2'-bis(o-methoxyphenyl)-4,4',5,5'-tetraphenyl-biimidazole, phenyl)-4,4',5,5'-tetraphenyl-biimidazole), 2,2'-bis(o-ethylphenyl)-4,4',5,5'-tetraphenyl-biimidazole), 2,2'-bis(p-methoxyphenyl)-4,4',5,5'-tetraphenyl-biimidazole), 2,2'-bis(2,2',4,4'-tetramethoxyphenyl)-4,4',5,5'-tetraphenyl-biimidazole, 5,5'-tetraphenylbiimidazole (2,2'-bis(2,2',4,4'-tetramethoxyphenyl)-4,4',5,5'-tetraphenyl-biimidazole), 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-biimidazole, or 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetra phenyl-biimidazole.
[0175] Preferably, the other photoinitiator (D-4) can be 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, 2-benzyl-2-nitrogen-dimethylamine-1-(4-morpholinophenyl)-1-butanone, 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyldiimidazole, or a combination of these compounds.
[0176] Other photoinitiators (D-4) of the present invention may further include the following compounds: benzophenone compounds such as thioxanthone, 2,4-diethylthioxanthanone, thioxanthone-4-sulfone, benzophenone, 4,4'-bis(dimethylamino)benzophenone, or 4,4'-bis(diethylamino)benzophenone; α-diketone compounds such as benzil or acetyl; acyloin compounds such as benzoin; benzoin methyl ether; acylphosphineoxide compounds such as bis-(2,6-dimethoxy-benzoyl)-2,4,4-trimethyl-benzyl-phosphine oxide; quinone compounds such as anthraquinone or 1,4-naphthoquinone; phenacyl chloride (phenacyl chloride) Halides such as tribromomethyl-phenylsulfone, tris(trichloromethyl)-s-triazine, and peroxides such as di-tertbutylperoxide. Among them, benzophenone compounds are preferred, and 4,4'-bis(diethylamino)benzophenone is the best.
[0177] The above-mentioned other photoinitiators (D-4) may be used alone or in combination of two or more.
[0178] Based on 100 parts by weight of the total usage of the alkali-soluble resin (B), the usage of the other photoinitiator (D-4) may be 0 to 99 parts by weight, preferably 5 to 95 parts by weight, and more preferably 10 to 90 parts by weight.
[0179] Based on 100 parts by weight of the total usage of the alkali-soluble resin (B), the usage of the photoinitiator (D) may be 10 to 100 parts by weight, preferably 15 to 90 parts by weight, and more preferably 20 to 80 parts by weight.
[0180] Solvent (E)
[0181] The preparation of the photosensitive resin composition of the present invention is usually to dissolve the components other than the pigment (A) in a solvent (E) to prepare a liquid composition, and then add the pigment (A) and mix them evenly. The solvent (E) should be selected to dissolve the alkali-soluble resin (B), the compound containing an ethylenically unsaturated group (C) and the photoinitiator (D), and should not react with the above components and have appropriate volatility.
[0182] In addition, the solvent (E) may be the same as the solvent used in the preparation of the alkali-soluble resin (B) described above, and will not be described in detail herein. Preferably, the solvent (E) is selected from propylene glycol methyl ether acetate, cyclohexanone or ethyl 3-ethoxypropionate. The solvent (E) may be used alone or in combination.
[0183] Based on 100 parts by weight of the total usage of the alkali-soluble resin (B), the usage of the solvent (E) is 500 parts by weight to 5000 parts by weight, preferably 800 parts by weight to 4500 parts by weight, and more preferably 1000 parts by weight to 4000 parts by weight.
[0184] Additives (F)
[0185] In a preferred embodiment of the present invention, the photosensitive resin composition may selectively include additives (F), such as fillers, polymer compounds other than the alkali-soluble resin (B), adhesion promoters, antioxidants, ultraviolet absorbers, and / or anti-agglomeration agents.
[0186] The additive (F) may be used alone or in combination, and may include but is not limited to fillers such as glass or aluminum; polymer compounds other than alkali-soluble resins (B) such as polyvinyl alcohol, polyethylene glycol monoalkyl ether or polyfluoroacrylate; vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(2-methoxyethoxy)silane, nitrogen-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, nitrogen-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidolpropyltrimethoxysilane, 3-cyclohexyloxysilane, Adhesion promoters such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, or 3-thiolpropyltrimethoxysilane; antioxidants such as 2,2-thiobis(4-methyl-6-tert-butylphenol) and 2,6-di-tert-butylphenol; ultraviolet absorbers such as 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorophenylazide or alkoxybenzophenone; and / or anti-agglomeration agents such as sodium polyacrylate.
[0187] Based on 100 parts by weight of the total amount of the alkali-soluble resin (B), the amount of the additive (F) is 0.1 to 10 parts by weight, preferably 0.3 to 7 parts by weight, and more preferably 0.5 to 4 parts by weight.
[0188] Method for manufacturing liquid crystal display device
[0189] The liquid crystal display device of the present invention is a device having a color filter manufactured by the above method. Specific examples of the liquid crystal display device include a color liquid crystal display device, an organic EL display device, or an electronic paper.
[0190] A color liquid crystal display device having a color filter produced by the method of the present invention can be, for example, constructed such that a driving substrate equipped with a thin film transistor (TFT) and another substrate equipped with the color filter of the present invention face each other via a liquid crystal layer. Alternatively, the color liquid crystal display device can also be constructed such that a substrate having the color filter of the present invention formed on the surface of a driving substrate equipped with a thin film transistor (TFT) and a substrate having an indium tin oxide (ITO) electrode formed face each other via a liquid crystal layer. The latter structure can further improve the aperture ratio, and has the advantage of obtaining a bright and high-precision liquid crystal display device.
[0191] The color liquid crystal display device has a backlight module. For example, a backlight module can be used that combines a fluorescent lamp such as a cold cathode fluorescent lamp (CCFL) and a scattering plate. In addition, a backlight module using a white light emitting diode (LED) as a light source can also be used. For white LEDs, for example, a white LED that mixes a red LED, a green LED and a blue LED to obtain white light; a white LED that mixes a blue LED, a red LED and a green light-emitting phosphor to obtain white light; a white LED that mixes a blue LED, a red light-emitting phosphor and a green light-emitting phosphor to obtain white light; a white LED that mixes a blue LED and a YAG-based phosphor to obtain white light; a white LED that mixes a blue LED, an orange light-emitting phosphor and a green light-emitting phosphor to obtain white light; or a white LED that mixes an ultraviolet LED, a red light-emitting phosphor, a green light-emitting phosphor and a blue light-emitting phosphor to obtain white light.
[0192] In a color liquid crystal display device having a color filter produced by the method of the present invention, an appropriate liquid crystal module of twisted nematic (TN) type, super twisted nematic (STN) type, in-plane switching (IPS) type, vertical alignment (VA) type, or optically compensated birefringence (OCB) type can be used.
[0193] The organic EL display element having the color filter produced by the method of the present invention can have an appropriate structure, and for example, the structure disclosed in Japanese Laid-Open Patent Publication No. JP-11-307242 can be mentioned.
[0194] The electronic paper having the color filter produced by the method of the present invention may have an appropriate structure, and for example, the structure disclosed in Japanese Laid-Open Patent Publication No. JP 2007-41169 may be mentioned.
[0195] The following embodiments are used to illustrate the application of the present invention, but they are not used to limit the present invention. Anyone skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. DETAILED DESCRIPTION
[0196] Preparation of alkali-soluble resin (B)
[0197] Synthesis Example B-1
[0198] A stirrer, a thermometer, a condenser and a nitrogen inlet are set on a four-necked conical flask, and nitrogen is introduced. Then, 100 parts by weight of propylene glycol methyl ether acetate (abbreviated as PGMEA) is added, and the temperature is raised to 100°C. Next, 10 parts by weight of methacrylic acid (abbreviated as MAA), 20 parts by weight of 3,4-epoxycyclohexylmethyl methacrylate (EC-MMA), 10 parts by weight of 2-methylglycidyl methacrylate (MGMA), 20 parts by weight of N-phenylmaleimide (abbreviated as N-PMI), 40 parts by weight of 2-hydroxyethyl methacrylate (abbreviated as HEMA), and 4.5 parts by weight of 2,2'-azobis-2-methylbutyronitrile (abbreviated as AMBN) are dissolved in 100 parts by weight of propylene glycol methyl ether acetate to obtain a mixed solution, and the mixed solution is dripped dropwise into the above four-necked conical flask within 2 hours. After reacting at 100°C for 6.5 hours, the alkali-soluble resin (B-1) of Synthesis Example B-1 was obtained.
[0199] Synthesis Example B-2 to Synthesis Example B-6
[0200] Synthesis Examples B-2 to B-6 are prepared by the same method as the preparation method of the alkali-soluble resin (B-1) of Synthesis Example B-1, except that the types and amounts of raw materials in the alkali-soluble resin and the reaction conditions are changed in Synthesis Examples B-2 to B-6. The formulas and reaction parameters are shown in Table 1, and are not described in detail here.
[0201] Preparation of photosensitive resin composition
[0202] Example 1
[0203] 100 parts by weight of the alkali-soluble resin (B-1) obtained in the above-mentioned Synthesis Example B-1, 5 parts by weight of CI Pigment Red 254 (hereinafter referred to as A-1), 20 parts by weight of EO-modified trimethylolpropane trimethacrylate (hereinafter referred to as C-1) and 10 parts by weight of 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone (hereinafter referred to as D-4-1), 500 parts by weight of propylene glycol methyl ether acetate (hereinafter referred to as E-1) were added, and the mixture was dissolved and mixed with a shaking stirrer to prepare the photosensitive resin composition of Example 1. The photosensitive resin composition was evaluated in the following evaluation method. The results are shown in Table 2.
[0204] Examples 2 to 24 and Comparative Examples 1 to 3
[0205] Examples 2 to 24 and Comparative Examples 1 to 3 use the same preparation method as the photosensitive resin composition of Example 1, except that Examples 2 to 24 and Comparative Examples 1 to 3 change the type and amount of raw materials in the photosensitive resin composition, and their formulations and evaluation results are shown in Table 2, respectively, and are not described in detail here. Comparative Example 3 uses the following evaluation method similar to that of Examples 1 to 24 and Comparative Examples 1 to 2 to evaluate the gradient angle, except that Comparative Example 3 uses a high-pressure mercury lamp instead of an ultraviolet light emitting diode as the light source of the exposure device.
[0206]
[0207]
[0208] Evaluation method
[0209] Gradient Angle
[0210] The photosensitive resin compositions prepared in Examples 1 to 24 and Comparative Examples 1 to 3 are coated on a 100 mm×100 mm glass substrate by spin coating. Then, reduced pressure drying is performed at a pressure of about 100 mmHg for about 30 seconds. Next, the glass substrate is pre-baked at 80°C for 2 minutes to form a pre-baked coating film with a film thickness of 2.5 μm. Afterwards, an ultraviolet light emitting diode that can emit a single-peak ultraviolet light with a wavelength of 365 nm is used as the light source of the exposure device for the pre-baked coating film of Examples 1 to 24 and Comparative Examples 1 to 2, and a high-pressure mercury lamp is used as the light source of the exposure device for the pre-baked coating film of Comparative Example 3. At 100 mJ / cm 2 After irradiating the pre-baked coating film with an exposure amount of, the exposed pre-baked coating film is immersed in a developer (0.04% potassium hydroxide) at 23°C for 60 seconds to remove the portion of the pre-baked coating film that has not been irradiated with ultraviolet light. Then, after washing with pure water, post-baking treatment is performed in an oven at 235°C for 30 minutes to obtain a pixel pattern. The gradient angle (angle between the glass substrate and the pattern) of the pixel pattern of each embodiment and comparative example is observed with a scanning electron microscope (manufactured by Hitachi, and model number is S-3000N), and evaluated according to the following criteria. The evaluation results are shown in Table 2.
[0211] ◎: 55°<gradient angle ≤ 70°;
[0212] ○: 45°<gradient angle ≤ 55°;
[0213] △: 35°<gradient angle ≦45°;
[0214] ╳: Gradient angle ≤ 35°, or gradient angle > 70°.
[0215] From the results in Table 2, we can see that if the illumination of the exposure process is not 50mW / cm 2 Up to 95mW / cm 2 When the photoinitiator (D) of the photosensitive resin composition comprises at least one of an oxime ester compound (D-1) as shown in formula (I), an oxime ester compound (D-2) as shown in formula (II), or an oxime ester compound (D-3) as shown in formula (III), the obtained pixel pattern has a better gradient angle.
[0216] It should be added that, although the present invention uses specific compounds, compositions, reaction conditions, processes, analysis methods or specific instruments as examples to illustrate the method for producing a pixel pattern, a color filter and its production method, and a liquid crystal display device of the present invention, anyone with ordinary knowledge in the technical field to which the present invention belongs will know that the present invention is not limited thereto. Without departing from the spirit and scope of the present invention, the method for producing a pixel pattern, a color filter and its production method, and a liquid crystal display device of the present invention may also be carried out using other compounds, compositions, reaction conditions, processes, analysis methods or instruments.
[0217] Although the present invention has been disclosed as above in the form of an implementation method, it is not intended to limit the present invention. Anyone with ordinary knowledge in the technical field to which the present invention belongs can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on what is defined in the claims.
Claims
1. A method for producing a pixel pattern, characterized in that: Include: Using a photosensitive resin composition to form a coating film on a substrate; as well as The coating film is exposed to light using an ultraviolet light emitting diode (UV-LED), the UV-LED having a peak wavelength of not less than 300 nm and an illumination of 50 mW / cm 2 Up to 95mW / cm 2 ;and The photosensitive resin composition comprises: Pigment (A); Alkali soluble resin (B); A compound (C) containing an ethylenically unsaturated group; a photoinitiator (D); and Solvent (E).
2. The method for producing a pixel pattern according to claim 1, characterized in that: The illumination of the exposure process is 52mW / cm 2 Up to 88mW / cm 2 .
3. The method for producing a pixel pattern according to claim 1, characterized in that: The photoinitiator (D) comprises an oxime ester compound (D-1) represented by the following formula (I): In formula (I), Y1 represents an organic group as shown in the following formula (I-1); Y2 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; Y3 represents an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an aryl group having 6 to 10 carbon atoms; In formula (I-1), Y4 represents a monovalent organic group; X1 represents an oxygen atom, a sulfur atom or a carbonyl group; and a represents an integer from 0 to 5.
4. The method for producing a pixel pattern according to claim 1, characterized in that: The photoinitiator (D) comprises an oxime ester compound (D-2) represented by the following formula (II): In formula (II), Z1 represents an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms, a phenyl group and a tolyl group; Z2 represents an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 4 to 10 carbon atoms or a substituted or unsubstituted phenyl group; Z3 represents a substituted or unsubstituted fluorenyl group or a substituted or unsubstituted carbazolyl group.
5. The method for producing a pixel pattern according to claim 1, characterized in that: The photoinitiator (D) comprises an oxime ester compound (D-3) represented by the following formula (III): In formula (III), R1, R2, R3, R4, R5, R6, R7 and R8 independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, COR 16 , a group represented by the following formula (III'-1); or R1 and R2, R2 and R3, R3 and R4, R5 and R6, R6 and R7 or R7 and R8 independently represent a group represented by the following formula (III'-2); However, the condition is that at least one pair of R1 and R2, R2 and R3, R3 and R4, R5 and R6, R6 and R7 or R7 and R8 is a group represented by formula (III'-2), R9, R 10 , R 11 and R 12 independently represent a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, wherein the alkyl group having 1 to 20 carbon atoms is unsubstituted or substituted by one or more of the following groups: halogen or phenyl; or R9, R 10 , R 11 and R 12 independently of one another represent unsubstituted phenyl or phenyl substituted by one or more of the following groups: alkyl having a carbon number of 1 to 6 or halogen; X2 represents CO or a single bond; R 13 represents an alkyl group having 1 to 20 carbon atoms, which is unsubstituted or substituted by one or more of the following groups: halogen, R 17 、COOR 17 OR 17 ; or R 13 represents an alkyl group having 2 to 20 carbon atoms, which is interrupted by one or more O or CO atoms, wherein the interrupted alkyl group having 2 to 20 carbon atoms is unsubstituted or substituted by one or more halogen atoms; or R 13 represents phenyl or naphthyl, each of which is unsubstituted or substituted with one or more of the following groups: an alkyl group having 1 to 20 carbon atoms or a haloalkyl group having 1 to 4 carbon atoms; R 14 represents a hydrogen atom, an alkoxy group having 1 to 20 carbon atoms, or an alkyl group having 1 to 20 carbon atoms; R 15 represents an aryl group having 6 to 20 carbon atoms, each of which is unsubstituted or substituted by one or more of the following groups: halogen, haloalkyl group having 1 to 4 carbon atoms, OR 17 , an alkyl group with a carbon number of 2 to 20 interrupted by one or more O; or each of which is substituted by an alkyl group with a carbon number of 1 to 20, the alkyl group with a carbon number of 1 to 20 is unsubstituted or substituted by one or more of the following groups: halogen, COOR 17 , phenyl or OR 17 ; or R 15 represents a hydrogen atom, a cycloalkyl group having 3 to 8 carbon atoms; or R 15 represents an alkyl radical having 1 to 20 carbon atoms, which is unsubstituted or substituted by one or more of the following groups: halogen or a cycloalkyl radical having 3 to 8 carbon atoms; R 16 represents an aryl group having 6 to 20 carbon atoms, each of which is unsubstituted or substituted by one or more of the following groups: halogen, haloalkyl group having 1 to 4 carbon atoms, OR 17 ; or each of them is substituted with one or more alkyl groups having a carbon number of 1 to 20, the alkyl group having a carbon number of 1 to 20 is unsubstituted or substituted with one or more of the following groups: halogen or OR 17 ; R 17 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, which is unsubstituted or substituted by one or more of the following groups: a halogen or a cycloalkyl group having 3 to 20 carbon atoms interrupted by one or more O atoms; or R 17 represents an alkyl group having 2 to 20 carbon atoms, in which one or more O atoms are interspersed; or R 17 represents phenyl, each of which is unsubstituted or substituted by one or more of the following groups: halogen, alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms; However, the condition is that there is at least one group represented by formula (III'-1) in the formula (III).
6. The method for producing a pixel pattern according to claim 1, characterized in that: Based on the total usage of the alkali-soluble resin (B) being 100 parts by weight, the usage of the pigment (A) is 5 to 300 parts by weight, the usage of the compound containing an ethylenically unsaturated group (C) is 20 to 200 parts by weight, the usage of the photoinitiator (D) is 10 to 100 parts by weight, and the usage of the solvent (E) is 500 to 5000 parts by weight.
7. The method for producing a pixel pattern according to claim 3, characterized in that: Based on 100 parts by weight of the total amount of the alkali-soluble resin (B), the amount of the oxime ester compound (D-1) is 1 part by weight to 100 parts by weight.
8. The method for producing a pixel pattern according to claim 4, characterized in that: Based on 100 parts by weight of the total amount of the alkali-soluble resin (B), the amount of the oxime ester compound (D-2) is 1 part by weight to 100 parts by weight.
9. The method for producing a pixel pattern according to claim 5, characterized in that: Based on 100 parts by weight of the total amount of the alkali-soluble resin (B), the amount of the oxime ester compound (D-3) is 1 part by weight to 100 parts by weight.
10. A method for manufacturing a color filter, characterized in that: The pixel pattern layer is formed by using the manufacturing method as claimed in any one of claims 1 to 9.
11. A color filter, characterized in that: It is prepared by the manufacturing method as claimed in claim 10.
12. A liquid crystal display device, characterized in that: Comprising the color filter as claimed in claim 11.
Citation Information
Patent Citations
Thermosetting composition
JP1991188153A
Heat resistant and radiation sensitive resin composition
JP1994192389A
Production of color filter, producing device therefor, color filter, liquid crystal display device and device equipped with this liquid crystal display device
JP1995318723A
Radiation-curable composition for producing dry film
JP1997005991A
Organic electroluminescent display device and its manufacture
JP1999307242A