Method for calculating dosage of ionic rare earth ore leaching agent

Through the Daonan model combining the surface potential and ion charge changes of rare earth ore samples, a leacher dosage calculation model for different ore soils and target leaching rates was established, which solved the problems of low recovery efficiency of rare earth resources and ammonia nitrogen pollution in the existing technology. , realize accurate determination of leachate dosage and low error rare earth resource recycling.

CN118942586AActive Publication Date: 2024-11-12JIANGXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202410979120.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The prior art fails to effectively calculate the amount of ionic rare earth ore leaching agent, resulting in low recovery efficiency of rare earth resources and ammonia nitrogen pollution, and failure to adapt to the conditions of different mineral soils, resulting in large error in the calculation of the amount of leaching agent.

Method used

By comprehensively considering the surface potential changes of rare earth ore and the effective charge changes of ammonium ions and lanthanum ions under different ionic strengths, the Daonan model is used to characterize the leaching process and establish the leaching at different ore soils and target leaching rates. Calculation model of single consumption of ammonium sulfate agent.

Benefits of technology

The calculation error of rare earth leaching rate is reduced, and the theoretical basis for determining the amount of leaching agent is provided. The actual error is only within 0.82%, which improves the efficiency of rare earth resource recovery and reduces ammonia nitrogen pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004955505130000031
    Figure BDA0004955505130000031
  • Figure BDA0004955505130000041
    Figure BDA0004955505130000041
  • Figure BDA0004955505130000049
    Figure BDA0004955505130000049
Patent Text Reader

Abstract

The invention discloses a method for calculating the dosage of an ionic rare earth ore leaching agent, and relates to the field of leaching beneficiation. The method for calculating the dosage of the ionic rare earth mineral leaching agent comprises the following steps: testing the charge density of the surface of pure lanthanum mineral; determining the content of ammonium ions and the content of lanthanum ions adsorbed by the solid phase of the pure lanthanum mineral, and determining the relationship between the relative effective charge coefficient of the lanthanum ions and the ammonium ions and the ion strength; determining the relationship between the Doosouth equilibrium selection coefficient and the ammonium ion activity in the supernate; and according to the ion activity coefficient, the Doosouth equilibrium selection coefficient and the ion exchange ratio of ammonium ions to lanthanum, carrying out fitting calculation to obtain the relationship between the unit consumption and the leaching rate of the mineral leaching agent ammonium sulfate. According to the ionic rare earth ore leaching agent dosage calculation method, the surface potential change of an ionic rare earth ore sample and the effective charge change conditions of ammonium ions and lanthanum ions under different ionic strengths are comprehensively considered, the ore leaching process is depicted through a Doognan model, and a calculation model for the unit consumption of the ore leaching agent ammonium sulfate under different ore soil and different target leaching rates is provided. And the calculation error of the rare earth leaching rate is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of leaching and mineral processing, and in particular to a method for calculating the dosage of an ionic rare earth leaching agent. Background Art

[0002] The rare earths in ionic rare earth ores are mainly adsorbed on clay minerals in the form of hydrated or hydroxyl hydrated ions, so they are mainly mined by chemical solution leaching. The amount of leaching agent used in the mining process is the main factor affecting the recovery rate of ionic rare earth ore resources. Excessive use of leaching agent will cause ammonia nitrogen pollution and increase production costs; too little leaching agent will result in low leaching efficiency and insufficient recovery of rare earth resources. Therefore, by describing the adsorption of leaching agent cations and the desorption process of rare earth ions, quantitatively characterizing the leaching mechanism and establishing a leaching agent dosage calculation model are of great significance for achieving efficient mining and protecting the mine environment.

[0003] At present, the industry has no standards for the research on the dosage of leaching agents, and most of them are based on field experience. The invention patent with the authorization announcement number CN107190144B discloses a method for calculating the dosage of ammonium sulfate for in-situ leaching of ionic rare earths. It is based on the chemical reaction equation of rare earth ions and ammonium ions, and uses the reaction equilibrium constant to establish a leaching agent dosage calculation model to calculate the minimum and maximum values ​​of ammonium sulfate unit consumption. The invention patent with the authorization announcement number CN111180017B discloses a method for calculating the dosage of ionic rare earth leaching agents. It uses a binary desorption equilibrium model to divide the ammonium consumption in leaching into three parts: ion exchange consumption, specific adsorption consumption, and consumption to maintain the concentration of leaching agents, and calculates the corresponding leaching agent dosage based on the DED model. The above schemes have a certain guiding role in calculating the amount of leaching agent, but they do not take into account that the essence of the ionic rare earth ore mining process is the adsorption / desorption of ions under the action of the electric field on the surface of the ore soil. As a result, the above calculations of the amount of ionic rare earth ore leaching agent do not reveal the essence of the desorption of rare earth ions and cannot adapt to the conditions of different ore properties in various places.

[0004] Therefore, a method is needed to calculate the unit consumption of leaching agents for different mineral soils and different target leaching rates. Summary of the invention

[0005] The purpose of the present application is to provide a method for calculating the dosage of an ionic rare earth leaching agent. By comprehensively considering the changes in the surface potential of ionic rare earth ore samples and the changes in the effective charges of ammonium ions and lanthanum ions under different ionic strengths, the Donan model is used to characterize the leaching process, and a calculation model for the unit consumption of leaching agent ammonium sulfate under different mineral soils and different target leaching rates is proposed to reduce the calculation error of the rare earth leaching rate.

[0006] This application is implemented as follows:

[0007] The present application provides a method for calculating the dosage of an ionic rare earth leaching agent, which comprises the following steps:

[0008] Calculate the charge density σ0 on the surface of pure lanthanum mineral;

[0009] Conduct adsorption and desorption tests on pure lanthanum minerals, measure the ammonium ion concentration and lanthanum ion concentration in the supernatant, and calculate the ammonium ion content adsorbed by the solid phase of pure lanthanum minerals and lanthanum ion content

[0010] Determine the relative effective charge coefficients of lanthanum and ammonium ions The relationship between the ammonium ion and the lanthanum ion exchange ratio ω was calculated.

[0011] Determination of Donan equilibrium selectivity k and ammonium ion activity in supernatant relationship;

[0012] According to the ion activity coefficient γ i The relationship between the unit consumption of ammonium sulfate and the leaching rate was obtained by fitting and calculating the Daonan equilibrium selectivity coefficient k and the exchange ratio of ammonium ions to lanthanum ions ω.

[0013] In some optional embodiments, pure lanthanum mineral is prepared using the following steps:

[0014] A predetermined mass of rare earth ore and lanthanum sulfate solution are mixed and stirred for 1-3 hours, followed by solid-liquid separation, and the above steps are repeated at least 3 times to obtain a sample;

[0015] The sample was washed with deionized water until the lanthanum ion concentration in the washing solution was lower than 0.005 mmol / L, and the sample was dried.

[0016] In some optional embodiments, testing the charge density on the surface of a pure lanthanum mineral comprises the following steps:

[0017] Test the ion phase of pure lanthanum minerals and the lanthanum ion grade Q c and specific surface area S;

[0018] The surface charge density of pure lanthanum minerals was calculated using the following formula;

[0019]

[0020] Where: σ0 is the surface charge density, C / m 2 ; For La 3+ The electricity price; Q c is the lanthanum ion grade in the ionic phase, g / g; F is the Faraday constant; is the relative molar mass of lanthanum ions, which is 138.91 g / mol; S is the specific surface area of ​​pure lanthanum mineral, m2 / g.

[0021] In some optional embodiments, the adsorption and desorption test of pure lanthanum mineral is carried out to obtain the ammonium ion content adsorbed by the solid phase of pure lanthanum mineral. and lanthanum ion content The following steps are involved:

[0022] Pure lanthanum mineral is added into ammonium sulfate solution of different concentrations and reacted at a preset temperature for 4-10 hours, followed by solid-liquid separation to obtain a supernatant;

[0023] The ammonium ion concentration and lanthanum ion concentration in the supernatant were measured respectively, and the ammonium ion activity in the supernatant was calculated. and lanthanum ion activity Calculation of the ammonium ion content adsorbed on the solid phase of pure lanthanum minerals and lanthanum ion content

[0024] In some alternative embodiments, the relative effective charge coefficients of lanthanum ions and ammonium ions are determined. The relationship with the ionic strength I includes the following steps:

[0025] The relative effective charge coefficients of lanthanum ions and ammonium ions were calculated using the following formula: and

[0026]

[0027] In the formula, and is the ammonium ion content and lanthanum ion content of pure lanthanum mineral solid phase adsorption, mol / g; β i is the relative effective charge coefficient of ion i; is the surface potential, V; and is the activity of ammonium ions and lanthanum ions in the supernatant, mol / L; R is the gas constant, which is 8.314 J / (mol·K); T is the absolute temperature, K; F is the Faraday constant; S is the specific surface area of ​​pure lanthanum mineral, m 2 / g; κ is the Debye parameter, nm -1 ; m is the coefficient related to the electrolyte type; ε is the leaching rate;

[0028] The following formulas were used for mathematical fitting to obtain the relative effective charge coefficients of lanthanum ions and ammonium ions. and Relationship with ionic strength I;

[0029] β=blnI+d;

[0030] Where: I is the ionic strength, mol / L; b and d are coefficients; β is the relative effective charge coefficient of lanthanum ion or ammonium ion.

[0031] In some optional embodiments, the ammonium ion and lanthanum ion exchange ratio ω is calculated using the following formula:

[0032]

[0033] Where: Z i is the charge of ion i; β i is the relative effective charge coefficient of ion i.

[0034] In some optional embodiments, determining the Donan model equilibrium selectivity coefficient k and ammonium ion activity The relationship includes the following steps:

[0035] According to the ammonium ion activity in the supernatant The following formula was used for mathematical fitting to obtain the equilibrium selectivity coefficient k of the Donan model and the ammonium ion activity in the supernatant: The relationship between:

[0036]

[0037] In the formula, k is the equilibrium selection coefficient of the Donan model; f is the coefficient; is the ammonium ion activity in the supernatant.

[0038] In some alternative embodiments, the ion activity coefficient γ i Calculated based on the ion hydration radius and ionic strength.

[0039] In some optional embodiments, according to the ion activity coefficient γ i , the Daonan equilibrium selectivity coefficient k and the exchange ratio of ammonium ions and lanthanum ions ω are used to calculate the relationship between the dosage of ammonium sulfate and the leaching rate:

[0040]

[0041] In the formula, is the dosage of ammonium sulfate, g / g; is the amount of initial ammonium ions, mol / g; is the molar mass of ammonium sulfate, g / mol; γ i is the activity coefficient of ion i; ω is the exchange ratio of ammonium ion to lanthanum ion; ε is the leaching rate, %; θ is the grade of rare earth ore, mol / g; m 矿 is the mass of rare earth ore, g; k is the Donan equilibrium selectivity coefficient.

[0042] The beneficial effect of the present application is that the method for calculating the dosage of the ionic rare earth leaching agent provided by the present application comprises the following steps: testing the charge density σ0 on the surface of the pure lanthanum mineral; conducting an adsorption and desorption test of the pure lanthanum mineral to obtain the ammonium ion content adsorbed by the solid phase of the pure lanthanum mineral; and lanthanum ion content Determine the relative effective charge coefficients of lanthanum and ammonium ions Relationship with ionic strength I; Determination of Donnan equilibrium selectivity coefficient k and ammonium ion activity in supernatant According to the ion activity coefficient γ i , the Daonan equilibrium selectivity coefficient k and the exchange ratio of ammonium ions and lanthanum ions ω are fitted and calculated to obtain the relationship between the unit consumption of ammonium sulfate and the leaching rate. The method for calculating the dosage of ionic rare earth leaching agents provided in this application comprehensively considers the changes in the surface potential of the ionic rare earth ore sample and the changes in the effective charge of ammonium ions and lanthanum ions under different ionic strengths. The Daonan model is used to characterize the leaching process, and a calculation model for the unit consumption of ammonium sulfate for different mineral soils and different target leaching rates is proposed, which provides a theoretical basis for the reasonable determination of the dosage of the leaching agent. The calculated rare earth leaching rate and the actual rare earth leaching rate have an error of only 0.82%. DETAILED DESCRIPTION

[0043] The embodiments described in this application are part of the embodiments of the present application, rather than all of the embodiments. Therefore, the detailed description of the embodiments of the present application provided below is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of this application.

[0044] The present application provides a method for calculating the dosage of an ionic rare earth leaching agent, which comprises the following steps:

[0045] Step 1: Prepare pure lanthanum mineral; Mix a predetermined mass of rare earth ore and lanthanum sulfate solution and stir for 1-3 hours, then separate the solid and liquid, repeat the above steps at least 3 times to obtain a sample; use deionized water to wash the sample until the lanthanum ion concentration in the washing solution is less than 0.005mmol / L, and dry the sample to obtain pure lanthanum mineral. Optionally, the rare earth ore and lanthanum sulfate solution are mixed in a mass ratio of 1:1, and the concentration range of the lanthanum sulfate solution is 0.005-0.020mol / L

[0046] Step 2: Test the charge density σ0 on the surface of pure lanthanum mineral;

[0047] Test the ion phase of pure lanthanum minerals and the lanthanum ion grade Q c and specific surface area S;

[0048] The surface charge density of pure lanthanum minerals was calculated using the following formula;

[0049]

[0050] Where: σ0 is the surface charge density, C / m 2 ; For La 3+ The electricity price; Q c is the lanthanum ion grade in the ionic phase, g / g; F is the Faraday constant; is the relative molar mass of lanthanum ions, which is 138.91 g / mol; S is the specific surface area of ​​pure lanthanum mineral, m 2 / g.

[0051] Step 3: Conduct adsorption and desorption tests on pure lanthanum minerals to obtain the ammonium ion content adsorbed by the solid phase of pure lanthanum minerals. and lanthanum ion content

[0052] Pure lanthanum mineral is added into ammonium sulfate solution of different concentrations and reacted at a preset temperature for 4-10 hours, followed by solid-liquid separation to obtain a supernatant;

[0053] The ammonium ion concentration and lanthanum ion concentration in each supernatant were measured respectively, and the ammonium ion activity in the supernatant was calculated. and lanthanum ion activity And calculate the ammonium ion content adsorbed by the solid phase of pure lanthanum minerals and lanthanum ion content

[0054] Step 4: Determine the relative effective charge coefficients of lanthanum and ammonium ions Relationship with ionic strength I;

[0055] The relative effective charge coefficients of lanthanum ions and ammonium ions were calculated using the following formula: and

[0056]

[0057] In the formula, and is the content of ammonium ions and lanthanum ions adsorbed on the solid phase of pure lanthanum minerals; β i is the relative effective charge coefficient of ion i, where ion i is ammonium ion or lanthanum ion; is the surface potential, V; and is the activity of ammonium ions and lanthanum ions in the supernatant, mol / L; R is the gas constant, which is 8.314 J / (mol·K); T is the absolute temperature, K; F is the Faraday constant; S is the specific surface area of ​​pure lanthanum mineral, m 2 / g; κ is the Debye parameter, I is the ionic strength; m is a parameter related to the electrolyte type; ε is the leaching rate;

[0058] The following formulas were used for mathematical fitting to obtain the relative effective charge coefficients of lanthanum ions and ammonium ions. and Relationship with ionic strength I;

[0059] β=blnI+d;

[0060] Where: I is the ionic strength, mol / L; b and d are coefficients; β is the relative effective charge coefficient of lanthanum ion or ammonium ion.

[0061] The exchange ratio ω of ammonium ions and lanthanum ions was calculated using the following formula:

[0062]

[0063] Where: Z i is the charge of ion i; β i is the relative effective charge coefficient of the i ion; the i ion is an ammonium ion or a lanthanum ion.

[0064] Step 5: Determine the Donnan equilibrium selectivity coefficient k and the ammonium ion activity in the supernatant relationship;

[0065] According to the adsorption amount of ammonium ions in the solid phase of pure lanthanum minerals and the activity of ammonium ions in the supernatant The Donan model equilibrium selectivity coefficient k and ammonium ion activity were obtained by mathematical fitting using the following formula: The relationship between:

[0066]

[0067] In the formula, k is the equilibrium selection coefficient of the Donan model; f is the coefficient, is the ammonium ion activity in the supernatant.

[0068] Step 6: According to the ion activity coefficient γ i The relationship between the unit consumption of ammonium sulfate and the leaching rate was obtained by fitting and calculating the Daonan equilibrium selectivity coefficient k and the exchange ratio of ammonium ions and lanthanum ions ω using the following fitting formula:

[0069]

[0070] In the formula, is the dosage of ammonium sulfate, g / g; is the amount of initial ammonium ions, mol / g; γ iis the activity coefficient of ion i; ω is the exchange ratio of ammonium ion to lanthanum ion; ε is the leaching rate, %; θ is the grade of rare earth ore, mol / g; m 矿 is the mass of rare earth ore, g; k is the Donan equilibrium selectivity coefficient.

[0071] The method for calculating the dosage of an ionic rare earth leaching agent provided in the embodiment of the present application comprehensively considers the changes in the surface potential of the ore sample during leaching in the ionic rare earth ore and the changes in the effective charge of ammonium ions and lanthanum ions at different ionic strengths, characterizes the leaching process with the Donan model, and proposes a calculation model for the unit consumption of ammonium sulfate, a leaching agent, for different rare earth ores and different target leaching rates, which provides a theoretical basis for reasonably determining the dosage of the leaching agent. The dosage of the leaching agent determined by the method for calculating the dosage of an ionic rare earth leaching agent provided in the embodiment of the present application is scientific and reasonable, and the error with the actual rare earth leaching rate is only within 0.82%.

[0072] Among them, according to the essence of the adsorption and desorption process of ions on the surface of rare earth ore, the leaching agent solution and rare earth ore are regarded as a Daonan system, the edge of the counter-ion adsorption layer in the double electric layer on the surface of the rare earth ore is set as the imaginary Daonan surface, and the inner side of the Daonan surface is regarded as the inner phase of the system, including the negatively charged rare earth ore colloid that cannot pass through the imaginary Daonan surface and the counter-ions adsorbed by the rare earth ore colloid; the outer side of the Daonan surface is the external phase of the system, which is a uniform leaching agent solution.

[0073] Therefore, the selectivity coefficient of ammonium ions and rare earth ions (lanthanum ions) in the mining process of ionic rare earth ores can be expressed as:

[0074]

[0075] Where: k is the Daonan equilibrium selection coefficient; σ i is the adsorption amount of ion i per unit mass on the mineral surface, mol / g; a i yes i Activity of ions in bulk solution, mol / L; Z i is the charge of ion i; β i is the relative effective charge coefficient of ion i; F is the Faraday constant, which is 9.65×10 4 C / mol; is the surface potential, V; R is the gas constant, which is 8.314 J / (mol·K); T is the absolute temperature, K.

[0076] The following relationship can be obtained by replacing the generated rare earth ion concentration (lanthanum ion), the generated ammonium ion adsorbate concentration and the consumed rare earth ion concentration with the expressions of rare earth concentration and rare earth ion leaching rate corresponding to the original ore grade:

[0077]

[0078] Where: is the amount of initial ammonium ions, mol / g; γ i is the activity coefficient of ion i; ω is the exchange ratio of ammonium ion to lanthanum ion; ε is the leaching rate, %; θ is the ore grade, mol / g; m 矿 is the mass of rare earth ore, g; k is the Donan equilibrium selectivity coefficient.

[0079] The above formula is the amount of ammonium ions required to extract a unit mass of ionic rare earth ore. By converting the above formula and units, the following calculation formula can be obtained:

[0080]

[0081] Where: is the dosage of ammonium sulfate, g / g; is the amount of initial ammonium ions, mol / g; γ i is the activity coefficient of ion i; ω is the exchange ratio of ammonium ion to lanthanum ion; ε is the leaching rate, %; θ is the ore grade, mol / g; m 矿 is the mass of rare earth ore, g; k is the Donan equilibrium selectivity coefficient.

[0082] The characteristics and performance of the method for calculating the dosage of the ionic rare earth leaching agent of the present application are further described in detail below in conjunction with the examples.

[0083] Example 1

[0084] The method for calculating the dosage of the ionic rare earth leaching agent provided in the embodiment of the present application was used to conduct a closed experiment in a rare earth mining area in southern Jiangxi. Ore samples from different locations were taken on site and mixed to prepare representative ionic rare earth ore samples. The ionic rare earth ore samples were subjected to adsorption and desorption tests to obtain key parameters, and column leaching tests were conducted using the calculated results as test conditions to verify the reliability of the calculated results.

[0085] Step 1, prepare pure lanthanum mineral; take a certain mass of rare earth ore, add an equal mass of 0.0125mmol / L lanthanum sulfate solution, stir for 2 hours for solid-liquid separation, repeat the above adding lanthanum sulfate solution, stirring and solid-liquid separation operation 3 times to obtain a sample, take deionized water to wash the water-soluble lanthanum ions on the surface of the sample until the lanthanum ion concentration in the washing solution is lower than 0.005mmol / L, and dry the washed sample at 70°C to obtain pure lanthanum mineral for use.

[0086] Step 2: Test the surface charge density of pure lanthanum minerals;

[0087] According to the existing technology, the ion phase of pure lanthanum minerals is tested for lanthanum ion grade Q c and its specific surface area S; its surface charge density σ0 is calculated according to the following formula (1).

[0088]

[0089] In formula (1): σ0 is the surface charge density, C / m 2 ; For La 3+ The electricity price; Q c is the lanthanum ion grade in the ionic phase, g / g; F is the Faraday constant; is the relative molar mass of lanthanum ions, which is 138.91 g / mol; S is the specific surface area of ​​pure lanthanum mineral, m 2 / g.

[0090] The lanthanum ion grade of the pure lanthanum mineral was 2.400 mg / g, and its specific surface area was 15.779 m 2 / g; According to formula (1), the surface charge density of pure lanthanum mineral is 0.317C / m 2 .

[0091] Step 3: Conduct adsorption and desorption tests on pure lanthanum minerals to obtain the ammonium ion content of the pure lanthanum mineral solid phase adsorption. and lanthanum ion content

[0092] Thirteen portions of pure lanthanum mineral prepared in step 2 were taken, and different concentrations of ammonium sulfate solution were added according to the solid-liquid mass ratio of 1:5. The ammonium ion concentrations of the added ammonium sulfate solution were 2mmol / L, 4mmol / L, 10mmol / L, 20mmol / L, 30mmol / L, 40mmol / L, 60mmol / L, 80mmol / L, 100mmol / L, 120mmol / L, 160mmol / L, 200mmol / L, 300mmol / L, etc., 13 groups of ammonium sulfate with different concentrations were added. The reaction was controlled at a certain temperature for 4 hours for solid-liquid separation, and the ammonium ion concentration and lanthanum ion concentration in the supernatant were measured respectively. The ionic strength I and the ammonium ion activity in the supernatant were calculated. and lanthanum ion activity Solid phase adsorption of ammonium ions and lanthanum ion content The results are shown in Table 1.

[0093] Table 1 Calculated ionic strength, ionic activity in supernatant and solid phase adsorbed ion content

[0094]

[0095] Step 4: Determine the relative effective charge coefficients of lanthanum ions and ammonium ions Relationship with ionic strength I;

[0096] The relative effective charge coefficients of lanthanum ions and ammonium ions were calculated using the following formula (2): and

[0097]

[0098] Substitute the ion concentration and ion content obtained in step 3 into the relative effective charge coefficient of lanthanum ion and ammonium ion calculated in formula (2): and The relative effective charge coefficients of lanthanum ions and ammonium ions were obtained by mathematical fitting using the following formula (3): and The relationship between the ionic strength I.

[0099] β=blnI+d (3)

[0100] Calculate the relationship between the relative effective charge coefficient of lanthanum ions and ammonium ions in pure lanthanum minerals and the ionic strength. The lanthanum ion is The ammonium ion is

[0101] Step 5: Determine the Donnan equilibrium selectivity coefficient k and the ammonium ion activity in the supernatant relationship;

[0102] According to the ion concentration obtained in step 3, calculate the ammonium ion activity in the supernatant The equilibrium selection coefficient k of the Donnan model is calculated and mathematically fitted by the following fitting formula (4):

[0103]

[0104] The Donnan model equilibrium selectivity coefficient k and ammonium ion activity are obtained The relationship between

[0105] Step 6: According to the ion activity coefficient γ i The relationship between the unit consumption of ammonium sulfate and the leaching rate was obtained by fitting and calculating the Daonan equilibrium selectivity coefficient k and the exchange ratio of ammonium ions and lanthanum ions ω using the following fitting formula:

[0106]

[0107] Determine the ammonium sulfate concentration to be 20 g / L and calculate the ion activity coefficient using formula (6): 0.147 is 0.719, and formula (6) is the existing Debye-Hückel limit formula; in formula (6), Z i is the charge of ion i, γ iis the ion activity coefficient of ion i, I is the ionic strength, B is a constant, which is 0.00328 at 25℃. is the ion volume parameter, which is approximately equal to the effective radius of the hydrated ion, 900 pm for lanthanum ions and 300 pm for ammonium ions; the ammonium ion activity in the supernatant is substituted into the fitting formula of step five, and the Donnan equilibrium selectivity coefficient k is calculated to be 0.666, and the exchange ratio of ammonium ions to lanthanum ions ω is 0.852. Substituting each parameter into formula (5) to obtain formula (7), formula (7) is the relationship between the unit consumption of ammonium sulfate and the leaching rate of the rare earth ore in the embodiment of the present application, and the unit consumption of ammonium sulfate can be calculated by substituting the corresponding leaching rate.

[0108]

[0109] The column leaching test was carried out on the ore sample in southern Jiangxi. The unit consumption of ammonium sulfate as the leaching agent was calculated by the model when the rare earth leaching rate was set to 80%, 85% and 90% respectively. The test used an ammonium sulfate solution with a concentration of 2% for leaching, and then injected with top water. Other specific parameters and test results are shown in Table 2. According to the calculation formula, for this mineral in southern Jiangxi, when the target rare earth leaching rate was 80%, 85% and 90%, the calculated unit consumption of ammonium sulfate was 4.48g / g, 5.46g / g and 7.45g / g as the amount of ammonium sulfate used in the column leaching process, and the actual leaching rate during column leaching was 80.66%, 85.69% and 90.30%. The maximum error between the calculated value and the measured value was 0.82%, indicating that the calculation method of the present invention is close to the actual situation and has a high practical value.

[0110] Table 2 Comparison of the leaching rate calculated in the present embodiment and the leaching rate obtained by actual leaching

[0111]

[0112] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

Claims

1. A method for calculating the dosage of an ionic rare earth leaching agent, characterized in that: It includes the following steps: Calculate the charge density σ0 on the surface of pure lanthanum mineral; Conduct adsorption and desorption tests on the pure lanthanum mineral, measure the ammonium ion concentration and lanthanum ion concentration in the supernatant, and calculate the ammonium ion content adsorbed by the pure lanthanum mineral in the solid phase. and lanthanum ion content Determine the relative effective charge coefficients of lanthanum and ammonium ions The relationship between the ammonium ion and the lanthanum ion exchange ratio ω was calculated. Determination of Donan equilibrium selectivity k and ammonium ion activity in supernatant relationship; According to the ion activity coefficient γ i The relationship between the unit consumption of ammonium sulfate and the leaching rate was obtained by fitting and calculating the Daonan equilibrium selectivity coefficient k and the exchange ratio of ammonium ions to lanthanum ions ω.

2. The method for calculating the dosage of an ionic rare earth leaching agent according to claim 1, characterized in that: The pure lanthanum mineral is prepared by the following steps: A predetermined mass of rare earth ore and lanthanum sulfate solution are mixed and stirred for 1-3 hours, followed by solid-liquid separation, and the above steps are repeated at least 3 times to obtain a sample; The sample was washed with deionized water until the lanthanum ion concentration in the washing solution was lower than 0.005 mmol / L, and the sample was dried.

3. The method for calculating the dosage of the ionic rare earth leaching agent according to claim 1, characterized in that: Testing the charge density of the surface of pure lanthanum minerals involves the following steps: Testing the ion phase lanthanum ion grade Q of the pure lanthanum mineral c and specific surface area S; The surface charge density of the pure lanthanum mineral is calculated using the following formula: Where: σ0 is the surface charge density, C / m 2 ; For La 3+ The electricity price; Q c is the lanthanum ion grade in the ionic phase, g / g; F is the Faraday constant; is the relative molar mass of lanthanum ions, which is 138.91 g / mol; S is the specific surface area of ​​pure lanthanum mineral, m 2 / g.

4. The method for calculating the dosage of an ionic rare earth leaching agent according to claim 1, characterized in that: The adsorption and desorption test of pure lanthanum minerals was carried out to obtain the ammonium ion content adsorbed by the solid phase of pure lanthanum minerals. and lanthanum ion content The following steps are involved: Adding the pure lanthanum mineral to ammonium sulfate solutions of different concentrations and reacting at a preset temperature for 4-10 hours, followed by solid-liquid separation to obtain a supernatant; The ammonium ion concentration and the lanthanum ion concentration in the supernatant are measured respectively, and the ammonium ion activity in the supernatant is calculated. and lanthanum ion activity Calculate the ammonium ion content of the pure lanthanum mineral solid phase adsorption and lanthanum ion content 5. The method for calculating the dosage of ionic rare earth leaching agent according to claim 3, characterized in that: Determine the relative effective charge coefficients of lanthanum and ammonium ions The relationship with the ionic strength I includes the following steps: The relative effective charge coefficients of lanthanum ions and ammonium ions were calculated using the following formula: and In the formula, and is the ammonium ion content and lanthanum ion content of pure lanthanum mineral solid phase adsorption, mol / g; β i is the relative effective charge coefficient of ion i; is the surface potential, V; and is the activity of ammonium ions and lanthanum ions in the supernatant, mol / L; R is the gas constant, which is 8.314 J / (mol·K); T is the absolute temperature, K; F is the Faraday constant; S is the specific surface area of ​​pure lanthanum mineral, m 2 / g; κ is the Debye parameter, nm -1 ; m is the coefficient related to the electrolyte type; ε is the leaching rate; The following formulas were used for mathematical fitting to obtain the relative effective charge coefficients of lanthanum ions and ammonium ions. and Relationship with ionic strength I; β=blnI+d; Where: I is the ionic strength, mol / L; b and d are coefficients; β is the relative effective charge coefficient of lanthanum ion or ammonium ion.

6. The method for calculating the dosage of ionic rare earth leaching agent according to claim 5, characterized in that: The exchange ratio ω of ammonium ions and lanthanum ions was calculated using the following formula: Where: Z i is the charge of ion i; β i is the relative effective charge coefficient of ion i.

7. The method for calculating the dosage of ionic rare earth leaching agent according to claim 5, characterized in that: Determination of the equilibrium selectivity coefficient k of the Donan model and the activity of ammonium ions The relationship includes the following steps: According to the ammonium ion activity in the supernatant The following formula was used for mathematical fitting to obtain the equilibrium selectivity coefficient k of the Donan model and the ammonium ion activity in the supernatant: The relationship between: In the formula, k is the equilibrium selection coefficient of the Donan model; f is the coefficient; is the ammonium ion activity in the supernatant.

8. The method for calculating the dosage of ionic rare earth leaching agent according to claim 1, characterized in that: The ion activity coefficient γ i Calculated based on the ion hydration radius and ionic strength.

9. The method for calculating the dosage of ionic rare earth leaching agent according to claim 1, characterized in that: According to the ion activity coefficient γ i , the Daonan equilibrium selectivity coefficient k and the exchange ratio of ammonium ions and lanthanum ions ω are used to calculate the relationship between the dosage of ammonium sulfate and the leaching rate: In the formula, is the dosage of ammonium sulfate, g / g; is the amount of initial ammonium ions, mol / g; is the molar mass of ammonium sulfate, g / mol; γ i is the activity coefficient of ion i; ω is the exchange ratio of ammonium ion to lanthanum ion; ε is the leaching rate, %; θ is the grade of rare earth ore, mol / g; m 矿 is the mass of rare earth ore, g; k is the Donan equilibrium selectivity coefficient.

Citation Information

Patent Citations

  • Calculation method for the dosage of ammonium sulfate in ionic rare earth in-situ leaching

    CN107190144B

  • Calculation method for dosage of ion-type rare earth leaching agent

    CN111180017B

  • Ore leaching liquid for ionic rare earth ore as well as use method thereof

    CN109161683A

  • Method for calculating dosage of ionic rare earth ore leaching agent

    CN111180017A

  • Method for determining source sink term in ionic type rare earth ore leaching process

    US20200199708A1

Cited By

  • Rare earth electrolyte solution activity coefficient prediction method based on machine learning

    CN120452565A