Manufacturing method of embedded chip substrate and temporary bonding structure
By using temporary bonding structure and precuring technology in the manufacturing process of embedded substrates in the chip, the problems of substrate warping and resin cracking are solved, and the bonding force between the chip and resin and the reliability of buried substrates are improved.
Patent Information
- Application Number
- CN202310531881.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-11
AI Technical Summary
In the existing method of manufacturing embedded substrates in chips, the substrate is prone to warping after landfilling the resin, resulting in resin cracking and chip interface separation, affecting reliability.
Using a temporary bonding structure, multiple temporary bonding and debonding are performed by setting a foam film and a support film on the substrate, and combining with the precuring step, a symmetric resin layer structure is formed to avoid warping and resin cracking.
It effectively reduces the warpage of the substrate, enhances the bonding force between the resin and the chip, and improves the reliability and stability of the buried substrate.
Smart Images

Figure CN118943027A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor packaging, and in particular to a manufacturing method of an embedded chip substrate and a temporary bonding structure. Background Art
[0002] Embedding the chip in the substrate is an advanced packaging form. By embedding the bare chip in the substrate, the signal transmission distance between the chip and the packaging components on the substrate surface and between chips can be greatly reduced, the signal transmission loss can be reduced, and the signal transmission quality can be improved; at the same time, the package size can be reduced and the device usage space can be compressed.
[0003] At present, the main manufacturing method of embedded chip substrate is to dig a cavity in the core board of the printed circuit board, embed the bare chip, fill it with resin, and then perform multi-layer wiring on both sides of the core board to form a substrate.
[0004] In the existing chip embedded substrate manufacturing method, after one side of the substrate is filled with resin and then subjected to single-sided pressing, severe warping is prone to occur due to the asymmetry of the structure. During the insulation layer pressing and curing baking process on the other side of the substrate, the substrate is flattened again, so that the substrate forms repeated bends from warping to flattening. Due to the high modulus of the solidified embedded resin, excessive warping and flattening will cause the rigid resin to crack. The rigid embedded resin and chip interface have weak bonding strength, which will also cause interface cracking. Resin cracking and chip interface separation may cause the embedded substrate to fail, and even when the embedded substrate is in a humid environment, water vapor is enriched at the crack interface, leading to serious reliability problems such as burning of the embedded substrate. Therefore, how to reduce substrate warping during substrate processing and manufacturing is a technical problem in the processing and manufacturing of embedded substrates, and an important issue in improving the reliability of embedded substrates. Summary of the invention
[0005] The object of the present invention is to provide a method for manufacturing an embedded chip substrate and a temporary bonding structure.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for manufacturing an embedded chip substrate comprises the following steps:
[0008] A substrate window is provided, wherein a cavity for accommodating the chip is provided on the substrate, and two surfaces of the substrate are respectively a first bonding surface and a resin embedding surface;
[0009] A first temporary bonding, bonding a first bonding material layer to the first bonding surface, wherein the first bonding material layer comprises a foaming film, a support film and a pressure-sensitive adhesive film stacked in sequence, and the foaming film of the first bonding material layer is bonded to the substrate, and a first support plate is fixed to a side of the first bonding material layer away from the substrate;
[0010] Attaching the chip, placing the chip in the accommodating cavity;
[0011] A first pressing and embedding resin, wherein the embedding resin is pressed and embedded on the embedding resin surface of the substrate to form a first resin layer, wherein a side of the first resin layer facing away from the substrate is a second bonding surface;
[0012] Second temporary bonding, bonding a second bonding material layer to the second bonding surface, wherein the second bonding material layer comprises a foaming film, a support film and a pressure-sensitive adhesive film stacked in sequence, and the foaming film of the second bonding material layer is bonded to the first resin layer, and a second support plate is fixed to a side of the second bonding material layer away from the first resin layer, and performing a first pre-curing;
[0013] A first debonding step is to debond the foaming film and the first bonding surface of the first bonding material layer to remove the first bonding material layer and the first support plate;
[0014] Secondary pressing and embedding resin, pressing and embedding resin on the first bonding surface of the substrate to form a second resin layer, and performing a second pre-curing;
[0015] second debonding, debonding the foamed film of the second bonding material layer from the first resin layer to remove the second bonding material layer and the second support plate;
[0016] Blind hole processing, opening blind holes on the upper and lower surfaces of the structure formed in the previous step;
[0017] Circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step;
[0018] Resin insulation layer processing, in which a resin insulation layer is provided on both the upper surface and the lower surface of the structure formed in the previous step, and pre-cured;
[0019] To make an intermediate circuit, repeat the steps of blind hole processing, circuit production and resin insulation layer processing N times, N ≥ 0, to form an N-layer intermediate circuit, and no pre-curing is performed in the N-th resin insulation layer processing step, and pre-curing is performed after copper foil is pressed on the surface of the resin insulation layer formed in the N-th resin insulation layer processing step, so that the resin insulation layer in the formed structure is cured to more than 50%;
[0020] Curing: the structure formed in the previous step is placed in a laminator, clamped by a mirror steel plate, under a preset vacuum degree and a preset pressure, so that the resin in the structure is cured to more than 90%;
[0021] Manufacturing the outer layer circuit, performing blind hole processing and circuit manufacturing steps on the cured structure to form the outer layer circuit;
[0022] Making a solder resist layer, making a solder resist layer on the surface of the outer layer circuit;
[0023] A coating is applied on the surface of the structure formed after the solder resist layer is made.
[0024] In one implementation, the first debonding further includes the following steps: first cleaning, cleaning the first bonding surface; and / or,
[0025] After the second debonding, the method further includes a second cleaning step of cleaning the second bonding surface.
[0026] In one implementation, the first pre-curing is specifically: curing the resin in the structure formed in this step to more than 50%; or, the first pre-curing is specifically: placing the structure formed in this step in a constant temperature environment of 130°C-150°C for 30min-60min to pre-cure the resin in the structure.
[0027] In one implementation, the second pre-curing is specifically: curing the resin in the structure formed in this step to a degree of curing of more than 80%; or, the second pre-curing is specifically: placing the structure formed in this step in a constant temperature environment of 170°C-185°C for 25min-35min to pre-cure the resin in the structure.
[0028] In one implementation, the pre-curing in the resin insulation layer processing step is specifically: curing the resin insulation layer in the structure to a degree of 70%-80%; or, the pre-curing in the resin insulation layer processing step is specifically: placing the formed structure in a constant temperature environment of 95°C-105°C for 25min-35min, and then placing it in a constant temperature environment of 170°C-185°C for 25min-35min.
[0029] In one implementation, the raw materials used in the first pressing and filling resin step, the second pressing and filling resin step, and the insulating layer processing step are all ABF resin sheets, and the ABF resin sheet includes an ABF main layer, an OPP film attached to the first side of the ABF main layer, and a PET film attached to the second side of the ABF main layer.
[0030] In one implementation, the first resin embedding step is specifically: removing the OPP film of the ABF resin sheet, and laminating the first side of the ABF resin sheet on the embedding resin surface of the substrate to form a first resin layer, and performing a first pre-curing so that the resin in the structure formed in this step is cured to more than 50%, and the side of the first resin layer away from the substrate is the second bonding surface and retains the PET film; and / or,
[0031] The second pressing and filling resin step is specifically to remove the OPP film of the ABF resin sheet, and press the first side of the ABF resin sheet onto the first bonding surface of the substrate to form a second resin layer, and perform a second pre-curing to cure the resin in the structure formed in this step to more than 70%, and the second resin layer retains the PET film.
[0032] In one implementation, the curing temperature of the first pre-curing is lower than the debonding temperature of the first bonding material layer; or,
[0033] The debonding temperature of the first bonding material layer is lower than the debonding temperature of the second bonding material layer.
[0034] A temporary bonding structure, comprising:
[0035] A substrate, wherein the substrate is provided with a receiving cavity for receiving the chip, and two surfaces of the substrate are respectively a first bonding surface and a resin embedding surface;
[0036] A chip, wherein the chip is disposed in the accommodating cavity;
[0037] A first bonding material layer and a first supporting plate, wherein the first bonding material layer is bonded to the first bonding surface, the first bonding material layer comprises a foaming film, a supporting film and a pressure-sensitive adhesive film stacked in sequence, the foaming film of the first bonding material layer is bonded to the substrate, and the first supporting plate is bonded to the pressure-sensitive adhesive film of the first bonding material layer;
[0038] A first resin layer, the first resin layer is located on the buried resin surface of the substrate, and a side of the first resin layer facing away from the substrate is a second bonding surface;
[0039] A second bonding material layer and a second supporting plate, the second bonding material layer is bonded to the second bonding surface, the second bonding material layer comprises a foaming film, a supporting film and a pressure-sensitive adhesive film stacked in sequence, the foaming film of the second bonding material layer is bonded to the first resin layer, and the second supporting plate is bonded to the pressure-sensitive adhesive film of the first bonding material layer.
[0040] In one implementation, the back side of the chip is bonded to the foam film of the first bonding material layer.
[0041] In one implementation, the first support plate and / or the second support plate is a double-sided copper-clad plate, a metal plate, a glass plate or a ceramic plate; and / or the thickness of the first support plate and / or the second support plate is greater than 0.2 mm.
[0042] In the manufacturing method of the embedded chip substrate provided in the above embodiment, the foaming film of the first bonding material layer is bonded to the first bonding surface of the substrate, and the foaming film of the second bonding material layer is bonded to the first resin layer, which can avoid contamination caused by the pressure-sensitive adhesive. In the process of debonding, in the first debonding step, it is only necessary to heat to the debonding temperature of the foaming film of the first bonding material layer, and in the second debonding step, it is only necessary to heat to the debonding temperature of the foaming film of the second bonding material layer, so that the foaming film is separated from the substrate or the first resin layer. Compared with the pressure-sensitive adhesive film and the substrate or the first resin layer, contamination caused by the pressure-sensitive adhesive can be avoided, and debonding is easier.
[0043] In the above embodiment, the chip is preferably placed in the accommodating cavity, and the back of the chip is bonded to the foam film of the first bonding material layer. The back of the chip is the side of the chip away from its pad, and the front of the chip is the side with the pad. That is, the side of the chip away from the pad is bonded to the foam film of the first bonding material layer. After the first debonding is completed, the temporary bonding glue residue generated during the debonding process of the foam film is removed by cleaning. Cleaning includes water washing, ultrasonic water washing, and debonding in a debonding tank to effectively remove the temporary bonding glue residue on the surface of the substrate and the temporary bonding glue residue on the back of the chip. If the chip has a side with a pad bonded to the foam film of the first bonding material layer, the debonding treatment in the debonding tank cannot be used, and more stringent cleaning is required, and the cleaning process is more complicated. Therefore, it is preferred that the back of the chip is bonded to the foam film of the first bonding material layer.
[0044] In addition, in the manufacturing method of the embedded chip substrate provided by the above embodiment, the first pre-curing is performed after the first pressing and embedding of the resin, and the second pre-curing is performed after the second pressing and embedding of the resin. After each resin insulation layer is processed, only pre-curing is performed, but no complete curing is performed. After the intermediate circuit is completed, the resin curing degree in the structure is below 80%, and after all the resin layers are processed, another curing is performed. In this curing step, the resin layer in the formed structure is cured to more than 90%, that is, the resin curing degree in the structure after the curing step is more than 90%. In other words, in this application, a pre-curing is performed after each resin layer is processed, which is not a complete curing, but after all the resin layers are processed, another curing is performed to achieve a curing degree of more than 90%. In the manufacturing method of the embedded chip substrate, before the symmetrical structure is formed, the resin in the structure is in an incompletely cured state, so that the low warping state can be maintained, and the symmetrical structure is formed and then cured to more than 90%, which can effectively avoid resin cracking.
[0045] The present invention further provides a temporary bonding structure. The beneficial effects of the temporary bonding structure provided by the present invention are the same as the beneficial effects of the method for manufacturing the embedded chip substrate described in the above technical solution, and will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0047] Figure 1 A schematic flow chart of a method for manufacturing an embedded chip substrate provided by an embodiment of the present invention;
[0048] Figure 2 The structure formed after the substrate window opening step provided in the embodiment of the present invention;
[0049] Figure 3 A structure formed after the first temporary bonding step provided by an embodiment of the present invention;
[0050] Figure 4 The structure formed after the chip attaching step provided in the embodiment of the present invention;
[0051] Figure 5 The structure formed after the first pressing and embedding resin step provided in the embodiment of the present invention;
[0052] Figure 6 A structure formed after the second temporary bonding step provided by an embodiment of the present invention;
[0053] Figure 7 A structure formed after the first debonding step provided in an embodiment of the present invention;
[0054] Figure 8 The structure formed after the second pressing and embedding resin step provided in the embodiment of the present invention;
[0055] Fig. 9 A structure formed after the second debonding step provided in an embodiment of the present invention;
[0056] Fig.10 The structure formed after the blind hole processing step provided in the embodiment of the present invention;
[0057] Fig.11 A structure formed after the circuit manufacturing steps provided in the embodiment of the present invention;
[0058] Fig.12 The structure formed after the first resin insulation layer processing step provided by the embodiment of the present invention;
[0059] Fig.13 A structure formed after repeating the circuit manufacturing steps provided in an embodiment of the present invention;
[0060] Fig.14 The structure formed after the second resin insulation layer processing step provided by the embodiment of the present invention;
[0061] Fig.15 The structure formed after the step of making the outer layer circuit provided in the embodiment of the present invention;
[0062] Fig.16 The structure formed after the step of making the solder resist layer provided in the embodiment of the present invention;
[0063] Fig.17 A schematic structural diagram of a first bonding material layer or a second bonding material layer provided in an embodiment of the present invention.
[0064] Figure markings: 1-substrate, 1a-accommodating cavity, 1b-substrate circuit, 2-first bonding material layer, 3-first supporting plate, 4-chip, 5-first resin layer, 6-second bonding material layer, 7-second supporting plate, 8-second resin layer, 9-blind hole, 10-circuit outside the resin layer, 11-first resin insulating layer, 12-circuit outside the first resin insulating layer, 13-second resin insulating layer, 14-outer circuit, 15-solder mask, a-foaming film, b-support film, c-pressure-sensitive adhesive film. DETAILED DESCRIPTION
[0065] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0066] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0067] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.
[0068] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0069] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0070] See also Figure 1 , Figure 1 The flowchart of the embodiment provided by the present invention, the manufacturing method of the embedded chip substrate in the embodiment comprises the steps of:
[0071] S1: a window is opened on the substrate 1, and a receiving cavity 1a for receiving the chip 4 is opened on the substrate 1, and two surfaces of the substrate 1 are respectively a first bonding surface and a resin embedding surface;
[0072] In this step, the surface of the substrate 1 may or may not have circuits. Figure 2 The middle substrate has a substrate circuit 1b. Specifically, the substrate 1 can be a resin substrate 1 with no circuit on the surface or a double-sided copper-clad board with no circuit on the surface. Of course, copper circuits can also be set on the surface of the substrate 1. The accommodating cavity 1a opened on the substrate 1 can be a through hole that runs through the thickness direction of the substrate 1. The two sides of the substrate 1 are respectively a first bonding surface and a buried resin surface. Specifically, the two sides of the substrate 1 along the thickness direction of the substrate 1 are respectively the first bonding surface and the buried resin surface, or when the substrate 1 is placed horizontally, that is, when the thickness direction of the substrate 1 is along the vertical direction, the upper surface and the lower surface of the substrate 1 are respectively the buried resin surface and the first bonding surface. The structure formed after the window opening step of the substrate 1 is as follows. Figure 2 shown.
[0073] The substrate 1 may be a BT (Bismaleimide Triazine) resin substrate or a FR4 material substrate 1. BT resin material has a very high glass transition temperature, excellent dielectric properties, low thermal expansion coefficient, good mechanical characteristics and other properties, which are more suitable for the production of the substrate 1. FR4 is a code for a flame retardant material grade, which means that the resin material must be able to extinguish itself after burning. Of course, the substrate 1 can also be made of other materials, which are not limited here.
[0074] S2: first temporary bonding, bonding the first bonding material layer 2 to the first bonding surface, the first bonding material layer 2 comprising a foaming film a, a supporting film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the first bonding material layer 2 is bonded to the substrate 1, and a first supporting plate 3 is fixed to the side of the first bonding material layer 2 facing away from the substrate 1;
[0075] That is, the first bonding material layer 2 is bonded to the first bonding surface of the substrate 1. In this embodiment, the first bonding surface can be the lower surface of the substrate 1. The first bonding material layer 2 can include a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the first bonding material layer 2 is bonded to the substrate 1. A first supporting plate 3 is fixed to the side of the first bonding material layer 2 facing away from the substrate 1, and the pressure-sensitive adhesive film c of the first bonding material layer 2 is bonded to the first supporting plate 3, that is, the first bonding material layer 2 is located between the first supporting plate 3 and the substrate 1. The structure formed after the first temporary bonding step is as shown in FIG. Figure 3 shown.
[0076] It should be noted here that the first bonding material layer 2 can be first bonded to the first support plate 3 and then bonded to the substrate 1. In this way, the first bonding material layer 2 can be bonded to the first support plate 3 before the chip 4 is packaged for standby use. Of course, the first bonding material layer 2 can also be first bonded to the substrate 1 and then bonded to the first support plate 3, which is not limited here.
[0077] Among them, the material of the first support plate 3 can be BT resin, and the first support plate 3 can be a double-sided copper-clad plate made of BT resin. Of course, the first support plate 3 can also be other materials, which are not limited here. The thickness of the first support plate 3 can be greater than or equal to 0.2mm. Specifically, the thickness of the first support plate 3 can be 0.3mm, 0.4mm, 0.5mm, 0.6mm, etc. Further, the thickness of the first support plate 3 can be greater than or equal to 0.8mm, such as 0.8mm, 0.9mm, etc., so that the strength of the first support plate 3 can be ensured to prevent the substrate 1 from warping during processing.
[0078] In this embodiment, the first bonding material layer 2 can be 3195N temporary bonding adhesive produced by Nitto Corporation that is heat-foamed and debonded at 170° C., and of course other temporary bonding adhesives can be selected according to actual conditions, which is not limited here.
[0079] S3: attaching the chip 4, placing the chip 4 in the accommodating cavity 1a;
[0080] A chip 4 is arranged in the receiving cavity 1a of the substrate 1. The electrode side of the chip 4 can be oriented toward the side away from the first bonding material layer 2, that is, the electrode of the chip 4 is placed upward, or the electrode side of the chip 4 can be placed downward. When the receiving cavity 1a is a through hole, the chip 4 can contact the foaming film a of the first bonding material layer 2, and when the electrode side of the chip 4 is downward, its electrode contacts the foaming film a of the first bonding material layer 2. The structure formed after the chip 4 is attached is as follows: Figure 4 shown.
[0081] Preferably, when attaching the chip 4, the electrode side of the chip 4 can be oriented toward the side away from the first bonding material layer 2, that is, the electrode of the chip 4 faces upward, so that the foaming film of the first bonding material layer 2 does not contact the chip 4 electrode, but contacts the back of the chip 4, which can also prevent the chip electrode surface from being contaminated, causing contamination to cause contaminants to be buried in the substrate to form serious reliability problems. Alternatively, the surface insulation layer of the chip 4 also uses a resin with a protective film to prevent the chip electrode surface from being contaminated. The protective film can be a copper foil or a film of other materials.
[0082] S4: first pressing and filling resin, pressing and filling resin on the filling resin surface of the substrate 1 to form a first resin layer 5, and the side of the first resin layer 5 facing away from the substrate 1 is the second bonding surface;
[0083] That is, the embedding resin is pressed on the embedding resin surface of the substrate 1, and the embedded resin forms the first resin layer 5. In this embodiment, the embedding resin surface can be the upper surface of the substrate 1. Pressing the embedding resin on the embedding resin surface of the substrate 1 can be pressing the resin on the embedding resin surface of the substrate 1. Specifically, a vacuum laminating machine can be used to press the resin on the embedding resin surface of the substrate 1. During the process of pressing the embedding resin, the resin fills the gaps between the circuits on the surface of the substrate 1 and the gaps around the chip 4. The structure formed after the first step of pressing the embedding resin is as follows: Figure 5 shown.
[0084] There is a protective film on the surface of the first resin layer 5. In the second temporary bonding step, the foaming film of the second bonding material layer 6 is bonded to the protective film of the first resin layer 5. In this way, tearing off the protective film after debonding can prevent contamination.
[0085] In the first pressing and embedding resin step, an ABF (Ajinomoto Buildup Film) resin sheet may be selected. The ABF resin sheet includes an ABF layer, an OPP (O-phenylphenol) film attached to a first side of the ABF layer, and a PET (polyethylene glycol terephthalate) film attached to a second side of the ABF layer.
[0086] In the first resin embedding step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is laminated on the resin embedding surface of the substrate to form a first resin layer, and the side of the first resin layer facing away from the substrate is the second bonding surface and the PET film is retained. That is, in this step, the OPP film of the ABF resin sheet is torn off and the PET film is retained. The ABF resin sheet is laminated on the resin embedding surface of the substrate with one side of the OPP film removed.
[0087] Specifically, a vacuum laminator can be used for low-temperature vacuum lamination to press the ABF resin sheet with the OPP film removed onto the buried resin surface of the substrate. In this step, the ABF resin sheet is only bonded and leveled in the vacuum laminator. The vacuum laminator includes a vacuum laminating section and a leveling section. The vacuum laminating section is mainly used to press the ABF resin sheet onto the buried resin surface of the substrate. Since the surface of the inner layer circuit is uneven, the surface of the ABF resin sheet is still uneven after laminating by the vacuum laminating section, and then the leveling section levels the ABF resin sheet to make the surface of the ABF resin sheet flat.
[0088] The resin may be a GXT31 ABF resin sheet. Of course, the resin may also be a semi-cured PP (Prepreg) sheet or a copper-clad resin sheet RCC (Resin Coated Copper), which is not limited here.
[0089] S5: Second temporary bonding, bonding the second bonding material layer 6 to the second bonding surface, and a second support plate 7 is fixed to the side of the second bonding material layer 6 facing away from the first resin layer 5; the second bonding material layer 6 includes a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the second bonding material layer 6 is bonded to the first resin layer 5, specifically, the foaming film a of the second bonding material layer 6 is bonded to the protective film of the first resin layer 5, and the protective film can be a copper foil or a film of other materials. A second support plate 7 is fixed to the side of the second bonding material layer 6 facing away from the first resin layer 5, and the first pre-curing is performed in this step.
[0090] In this embodiment, the second bonding surface is the upper surface of the first resin layer 5. A second support plate 7 is fixed to the side of the second bonding material layer 6 facing away from the first resin layer 5, that is, the second bonding material layer 6 is located between the second support plate 7 and the first resin layer 5, and the second support plate 7 is bonded to the pressure-sensitive adhesive film c of the second bonding material layer 6. The structure formed after the second temporary bonding step is as shown in FIG. Figure 6 shown.
[0091] It should be noted here that the second bonding material layer 6 can be first bonded to the second support plate 7 and then bonded to the first resin layer 5. In this way, the second bonding material layer 6 can be bonded to the second support plate 7 before the chip 4 is packaged for standby use. Of course, the second bonding material layer 6 can also be first bonded to the first resin layer 5 and then bonded to the second support plate 7, which is not limited here.
[0092] After the second bonding material layer 6 is bonded to the second bonding surface, a first pre-curing is performed. The first pre-curing can be low-temperature thermal curing, so that the first resin layer 5 is cured to a certain extent, but not completely cured. The structure formed after the first pressing and embedding resin step is as shown in FIG. Figure 5 shown.
[0093] The first pre-curing may specifically be: placing the structure formed in this step in a constant temperature environment of 140° C. for 30 minutes. The first pre-curing is performed in an oven.
[0094] Among them, the material of the second support plate 7 can be BT resin, and the second support plate 7 can be a double-sided copper-clad plate made of BT resin. Of course, the second support plate 7 can also be made of other materials, which are not limited here. The thickness of the second support plate 7 can be greater than or equal to 0.2mm. Specifically, the thickness of the second support plate 7 can be 0.3mm, 0.4mm, 0.5mm, 0.6mm, etc. Further, the thickness of the second support plate 7 can be greater than or equal to 0.8mm, such as 0.8mm, 0.9mm, etc., so that the strength of the second support plate 7 can be ensured to prevent the substrate 1 from warping during processing.
[0095] In this embodiment, the second bonding material layer 6 can be 31950E temporary bonding adhesive produced by Nitto Corporation that foams and debonds at 210° C. Of course, other temporary bonding adhesives can be selected according to actual conditions, which is not limited here.
[0096] Since only the OPP film of the ABF resin sheet is torn off and the PET film is retained in step S4, the second bonding material layer 6 is directly bonded to the PET film of the first resin layer 5, thus avoiding the second bonding material layer 6 from directly contacting the ABF layer of the first resin layer 5. After subsequent debonding, the PET film is torn off to ensure that the first resin layer 5 is free from bonding contamination residues. The PET film can be torn off before or after the blind hole processing step.
[0097] S6: first debonding, debonding the foaming film a of the first bonding material layer 2 from the first bonding surface to remove the first bonding material layer 2 and the first support plate 3;
[0098] In this step, it is only necessary to debond the foaming film a of the first bonding material layer 2 from the first bonding surface of the substrate 1, that is, to remove the first bonding material layer 2 and the first support plate 3 from the substrate 1, while the foaming film a of the second bonding material layer 6 and the first resin layer 5 are not debonded, and the foaming film a of the second bonding material layer 6 is still bonded to the first resin layer 5. The first debonding can be a low-temperature debonding, and the debonding temperature of the first bonding material layer 2 is lower than the debonding temperature of the second bonding material layer 6. The structure formed after the first debonding step is as shown in FIG. Figure 7 shown.
[0099] The first pre-curing temperature should be lower than the debonding temperature of the first bonding material layer 2. If the debonding temperature of the first bonding material layer 2 is 170°C, the first pre-curing temperature should be lower than 170°C. Preferably, the first pre-curing temperature is lower than the debonding temperature of the first bonding material layer 2 by more than 10°C or 25°C-35°C. Specifically, the first pre-curing temperature is lower than the debonding temperature of the first bonding material layer 2 by 10°C, 15°C, 20°C, 25°C, 30°C, or 35°C. Preferably, the first pre-curing temperature may be lower than the debonding temperature of the first bonding material layer 2 by 20°C or 30°C.
[0100] S7: secondly press-filling the resin, press-filling the resin on the first bonding surface of the substrate 1 to form a second resin layer 8, and performing a second pre-curing;
[0101] That is, the embedding resin is pressed on the first bonding surface of the substrate 1, and the embedded resin forms the second resin layer 8. The embedding resin is pressed on the first bonding surface of the substrate 1, and the resin can be pressed on the first bonding surface of the substrate 1 by using a vacuum laminator. During the process of pressing the embedding resin, the resin fills the gaps between the circuits on the surface of the substrate 1 and the gaps around the chip 4.
[0102] After the first bonding surface of the substrate 1 is pressed and filled with resin, a second pre-curing is performed. The second pre-curing can be a low-temperature thermal curing, so that the second resin layer 8 is cured to a certain extent, but not completely cured. The structure formed after the second pressing and filling resin step is as follows Figure 8 As shown. It should be noted that during the second pre-curing process, the first resin layer 5 and the second resin layer 8 are further cured, and after the second pre-curing, the first resin layer 5 and the second resin layer 8 reach the same degree of curing, but the first resin layer 5 and the second resin layer 8 are not completely cured. The second pre-curing can be specifically: the structure formed in this step is placed in a constant temperature environment of 180°C for 30 minutes.
[0103] It should be noted that the thickness and / or material of the first resin layer 5 and the second resin layer 8 can be the same, so that the structures of the first resin layer 5 and the second resin layer 8 on the upper and lower surfaces of the substrate 1 are symmetrical, thereby reducing warping.
[0104] ABF (Ajinomoto Buildup Film) resin sheet can also be used in the second pressing and embedding resin step. In the second pressing and embedding resin step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is pressed on the first bonding surface of the substrate 1 to form a second resin layer 8, and a second pre-curing is performed, and the side of the second resin layer 8 facing away from the substrate retains the PET film. That is, in this step, the OPP film of the ABF resin sheet is torn off and the PET film is retained. The ABF resin sheet removes one side of the OPP film and is pressed on the first bonding surface of the substrate 1.
[0105] In this way, the PET film can protect the ABF layer, and the PET film can be torn off before or after the blind hole processing. The process of laminating the second resin layer 8 is also carried out in a vacuum laminator, and the second pre-curing is carried out in an oven, which will not be described in detail here.
[0106] In this step, the resin can be specifically selected from the ABF resin sheet of model GXT31. Of course, the resin can also be a semi-cured PP sheet or a copper-clad resin sheet RCC, which is not limited here.
[0107] S8 : second debonding, debonding the foaming film a of the second bonding material layer 6 and the first resin layer 5 to remove the second bonding material layer 6 and the second support plate 7 .
[0108] In this step, the foaming film a of the second bonding material layer 6 is debonded from the second bonding surface of the first resin layer 5, that is, the second bonding material layer 6 and the second support plate 7 are removed from the substrate 1. The structure formed after the second debonding step is as follows: Fig. 9 shown.
[0109] The debonding temperature of the second bonding material layer 6 should be higher than the debonding temperature of the first bonding material layer 2, and the debonding temperature of the second bonding material layer 6 may be 210°C. In addition, the second pre-curing temperature should be lower than the debonding temperature of the second bonding material layer 6. If the debonding temperature of the second bonding material layer 6 is 210°C, the second pre-curing temperature should be lower than 210°C. Preferably, the second pre-curing temperature is lower than the debonding temperature of the second bonding material layer 6 by more than 10°C or 25°C-35°C. Specifically, the second pre-curing temperature may be lower than the debonding temperature of the second bonding material layer 6 by 20°C or 30°C.
[0110] S9: blind hole 9 processing, blind holes 9 are opened on the upper surface and lower surface of the structure formed in the previous step. That is, blind holes 9 are opened on the upper surface and lower surface of the structure formed in the previous step of the blind hole 9 processing step. In this embodiment, blind holes 9 can be opened on the surface of the first resin layer 5 and the second resin layer 8, so that the circuits covered by the first resin layer 5 and the second resin layer 8 are electrically connected to the outer layer circuit 14 through the blind holes 9. Specifically, the blind holes 9 can be formed on the surface of the first resin layer 5 and the second resin layer 8 by laser drilling. The structure formed after the blind hole 9 processing step is as follows: Fig.10 shown.
[0111] S10: circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step;
[0112] Specifically, the upper and lower surfaces of the structure formed in the previous step are processed with circuits to form a circuit 10 outside the resin layer. In this embodiment, the circuit can be processed on the surface of the first resin layer 5 and the second resin layer 8, and the above circuit is electrically connected to the circuit covered by the first resin layer 5 and the second resin layer 8 through a blind hole 9. The structure formed after the circuit production step is as shown in FIG. Fig.11 shown.
[0113] S11: processing a resin insulation layer, providing a resin insulation layer on both the upper surface and the lower surface of the structure formed in the previous step, and pre-curing;
[0114] That is, the resin is pressed and filled on the upper and lower surfaces of the structure formed in the previous step to form a resin insulation layer on the upper and lower surfaces of the structure formed in the curing step. Specifically, the resin insulation layer formed in this step is the first resin insulation layer 11. The resin fills the gaps between the circuits formed in the circuit manufacturing step, and the first resin insulation layer 11 covers the circuits formed in the circuit manufacturing step and is partially in contact with the first resin layer 5 or the second resin layer 8. Pre-curing is performed, and this pre-curing is the third pre-curing, that is, the first resin insulation layer 11 is cured to a certain extent, but not completely cured. The structure formed after the first resin insulation layer processing step is as shown in FIG. Fig.12 shown.
[0115] The resin insulation layer can also be made of an ABF resin sheet. In the insulation layer processing step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is pressed on the upper surface and the lower surface of the structure formed in the previous step, and a third pre-curing is performed to cure the resin in the structure formed in this step to 70%-80%. A PET film is retained on the side of the insulation layer away from the substrate to protect the insulation layer from contamination.
[0116] In this step, the insulating layer resin can be specifically selected from the ABF resin sheet of model GXT31. Of course, the resin can also be a semi-cured PP sheet or a copper-clad resin sheet RCC, which is not limited here.
[0117] The third pre-curing may specifically be to place the formed structure in a constant temperature environment of 100° C. for 30 minutes, and then place it in a constant temperature environment of 180° C. for 30 minutes, so that the curing degree of the resin insulation layer reaches 70%-80%.
[0118] S12: Make an intermediate circuit, repeat the blind hole processing, circuit production and resin insulation layer processing steps N times, N ≥ 0, to form N layers of intermediate circuits, and do not pre-cure in the Nth resin insulation layer processing step, and pre-cure after pressing copper foil on the surface of the resin insulation layer formed in the Nth resin insulation layer processing step, so that the resin insulation layer in the formed structure is cured to more than 50%.
[0119] Among them, the steps of blind hole 9 processing, circuit manufacturing and resin insulation layer processing are repeated N times, and when N≥0 and N>0, N layers of intermediate circuits can be processed in this step. When N=0, the outer layer circuit is directly processed. That is, each time the steps of blind hole 9 processing, circuit manufacturing and resin insulation layer processing are repeated, a layer of intermediate circuit is processed. The key point in this embodiment is that, except for the Nth resin insulation layer processing step, in each of the other resin insulation layer processing steps, a pre-curing is performed after the resin insulation layer is set on the circuit surface, and the curing is not complete. The structure formed after the circuit manufacturing step is repeated is as follows: Fig.13 shown.
[0120] The insulating layer formed in the repeated first resin insulation layer processing step is the second resin insulation layer, the insulating layer formed in the repeated second resin insulation layer processing step is the third resin insulation layer, and so on. Similarly, the pre-curing in the repeated first resin insulation layer processing step is the fourth pre-curing, the pre-curing in the repeated second resin insulation layer processing step is the fifth pre-curing, and so on.
[0121] When the blind hole processing, circuit making and resin insulation layer processing steps are repeated once, the upper and lower surfaces of the structure formed in the previous step are pressed and filled with resin to form a second resin insulation layer 13, that is, the upper and lower surfaces of the structure formed in the repeated circuit making step are pressed and filled with resin to form a second resin insulation layer 13. Specifically, the resin fills the gaps between the circuits formed in the previous step, and the second resin insulation layer 13 covers the circuits formed in the circuit making step and partially contacts the first resin insulation layer 11. A fourth pre-curing is performed, that is, the resin in the structure is cured to a certain extent, but not completely cured. The structure formed after the second resin insulation layer processing step is as shown in FIG. Fig.14 The material of the second resin insulation layer 13 can also be ABF resin, and of course can also be PP (Prepreg semi-cured sheet) or copper-coated resin sheet RCC (Resin Coated Copper).
[0122] The fourth pre-curing may specifically be to place the formed structure in a constant temperature environment of 100° C. for 30 minutes, and then place it in a constant temperature environment of 180° C. for 30 minutes, so that the curing degree of the first resin insulation layer 11 reaches 70%-80%.
[0123] Furthermore, after the copper foil is pressed on the surface of the resin insulation layer formed in the Nth resin insulation layer processing step, pre-curing is performed to cure the resin insulation layer in the formed structure to more than 50%.
[0124] Specifically, the copper foil is laminated on the surface of the outermost resin insulating layer in the structure formed in the intermediate circuit manufacturing step. In this embodiment, the copper foil can be laminated on the upper and lower surfaces of the structure formed in the intermediate circuit manufacturing step. It should be noted that if the surface of the outermost resin layer in the structure formed in the previous step has a PET film, the PET film is removed, and then the copper foil is laminated, and then pre-curing is performed.
[0125] Alternatively, the resin insulation layer and the copper foil may be pressed together in the Nth resin insulation layer processing step, that is, when the last resin insulation layer is pressed, the last resin insulation layer and the copper foil are pressed together.
[0126] It should be noted that in the step of making the intermediate circuit S12, no pre-curing is performed after the resin insulation layer is pressed in the last resin insulation layer processing, or no pre-curing is performed in the Nth resin insulation layer processing, that is, the copper foil is directly pressed after the resin insulation layer is pressed, and then pre-curing is performed. In the step of making the intermediate circuit S12, except for the last resin insulation layer processing, pre-curing is performed after the resin insulation layer is pressed in the remaining N-1 resin insulation layer processing steps.
[0127] S13: Curing: the structure formed in the previous step is clamped by a mirror steel plate in a laminator, under a preset vacuum degree and a preset pressure, so that the resin in the structure is cured to more than 90%.
[0128] High temperature curing can be used in this step. After the step is completed, all resins in the structure are cured to more than 90%, that is, the first resin layer 5, the second resin layer 8, the first resin insulation layer 11 and the second resin insulation layer 13 can be cured to more than 90% or the degree of curing is more than 90%. Specifically, the resin in the formed structure is cured to more than 90% in an environment above 190°C. Specifically, the formed structure can be placed in a constant temperature environment above 190°C to cure the resin in the structure to more than 90%. For example, the formed structure can be placed in a constant temperature environment of 190°C or 195°C to cure the resin in the structure to more than 90%. Preferably, the formed structure is placed in a constant temperature environment of 190°C to cure the resin in the structure to more than 90%. In addition, the formed structure can also be placed in a constant temperature environment of 190°C-210°C to cure the resin in the structure to more than 90%.
[0129] Specifically, the formed structure can be placed in a laminator, and the structure formed in the previous step can be clamped with a mirror steel plate, and the resin in the structure can be cured to more than 90% under a preset vacuum degree and a preset pressure. Since the upper and lower surfaces of the laminator are mirror steel plates, under a vacuum environment, the substrate structure is leveled and cured at a relatively low pressure of 0.1MPa-0.7MPa and a temperature of 190℃-210℃ to maintain low warpage. The preset pressure is 0.1MPa-0.7MPa.
[0130] S14: manufacturing an outer layer circuit, performing blind hole processing and circuit manufacturing steps on the cured structure to form an outer layer circuit;
[0131] That is, blind hole processing and circuit manufacturing are performed on the upper and lower surfaces of the cured structure. In this embodiment, circuits are specifically processed on the upper and lower surfaces of the second resin insulating layer 13 to form an outer layer circuit 14. The structure formed after this step is as shown in FIG. Fig.15 shown.
[0132] S15: Making a solder resist layer, making a solder resist layer 15 on the surface of the outer layer circuit 14; the structure formed after the step of making the solder resist layer 15 is as follows Fig.16 shown.
[0133] S16: coating, coating the surface of the structure formed after the solder resist layer 15 is formed. The specific material of the coating can be NiPdAu (nickel palladium gold), NiAu (nickel gold), Sn (tin) or OSP (Organic Solderability Preservatives).
[0134] In the manufacturing method of the embedded chip substrate provided in the above embodiment, the foaming film of the first bonding material layer 2 is bonded to the first bonding surface of the substrate 1, and the foaming film a of the second bonding material layer 6 is bonded to the first resin layer 5, which can avoid the contamination caused by the pressure-sensitive adhesive. In the process of debonding, in the first debonding step, it is only necessary to heat to the debonding temperature of the foaming film a of the first bonding material layer 2, and in the second debonding step, it is only necessary to heat to the debonding temperature of the foaming film a of the second bonding material layer 6, so that the foaming film is separated from the substrate 1 or the first resin layer 5. Compared with the pressure-sensitive adhesive film and the substrate 1 or the first resin layer 5, the contamination caused by the pressure-sensitive adhesive can be avoided, and the debonding is easier.
[0135] In addition, in the manufacturing method of the embedded chip substrate provided by the above embodiment, the first pre-curing is performed after the first pressing and embedding of the resin, and the second pre-curing is performed after the second pressing and embedding of the resin. After each resin insulation layer is processed, only pre-curing is performed, but no complete curing is performed. After the intermediate circuit is completed, the resin curing degree in the structure is below 80%, and after all the resin layers are processed, another curing is performed. In this curing step, the resin layer in the formed structure is cured to more than 90%, that is, the resin curing degree in the structure after the curing step is more than 90%. In other words, in this application, a pre-curing is performed after each resin layer is processed, which is not a complete curing, but after all the resin layers are processed, another curing is performed to achieve a curing degree of more than 90%. In the manufacturing method of the embedded chip substrate, before the symmetrical structure is formed, the resin in the structure is in an incompletely cured state, so that the low warping state can be maintained, and the symmetrical structure is formed and then cured to more than 90%, which can effectively avoid resin cracking.
[0136] In addition, in the manufacturing method of the embedded chip substrate provided by the above embodiment, in the steps of attaching the chip 4, embedding the first resin layer and the second resin layer, the first support plate 3 and / or the second support plate 7 are used to support the substrate 1. The supporting function of the first support plate 3 and / or the second support plate 7 can reduce the overall warping of the substrate 1 caused by the asymmetric structure during the manufacturing process of the embedded chip substrate, ensuring that the substrate 1 is always in a low warping state during the entire manufacturing process of the embedded chip substrate. In addition, the first pre-curing is performed after the first pressing and embedding resin, and the second pre-curing is performed after the second pressing and embedding resin, so that the first resin layer 5 and the second resin layer 8 finally reach the same degree of curing, and the entire substrate 1 forms a symmetrical structure, which reduces the warping level of the substrate 1, avoids excessive warping of the substrate 1 caused by the different degrees of curing of the first resin layer 5 and the second resin layer 8 during the manufacturing process of the embedded chip substrate, and thus avoids the formation of brittle cured resin cracking and the chip 4 with weak bonding force and the resin interface cracking.
[0137] In addition, S6 can be added on the basis of the above embodiment. ,First cleaning step and / or S8 , Second washing step.
[0138] Specifically, in this embodiment, after the first debonding, the following step may be further included: S6 , The first cleaning is to clean the first bonding surface. That is, after the first bonding material layer 2 is debonded from the first bonding surface, the first bonding surface can be cleaned to prevent material residue. Specifically, a plasma cleaner can be used to clean the first bonding surface. Of course, other cleaning methods can also be used, such as degumming cleaning, which is not limited here. Specifically, the degumming can be carried out in a degumming tank at 70°C-85°C for 2-5 minutes to remove the residual foam film residue on the surface.
[0139] In addition, in this embodiment, the second debonding may further include the following steps: S8 , Second cleaning, cleaning the second bonding surface. That is, after the second bonding material layer 6 is debonded from the second bonding surface, the second bonding surface can be cleaned to prevent material residue. Specifically, a plasma cleaning machine can be used to clean the second bonding surface. Of course, other methods can also be used for cleaning, which is not limited here.
[0140] In the above embodiments, the first pre-curing may specifically include: curing the resin in the formed structure to more than 50%, that is, the curing degree of the resin after the first pre-curing is more than 50%, and the curing degree of the resin after the first pre-curing may be 60%, 70%, 75%, etc., so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. Preferably, the resin in the formed structure is cured to more than 70%, but not completely cured.
[0141] Alternatively, the first pre-curing may specifically include placing the formed structure in a constant temperature environment of 130° C. to 150° C. for 30 min to 60 min to pre-cure the resin in the structure. Specifically, the formed structure may be placed in a constant temperature environment of 130° C., 135° C., 140° C. or 150° C. for 30 min, 40 min or 50 min. Preferably, the formed structure is placed in a constant temperature environment of 140° C. for 60 min.
[0142] In addition, in each of the above embodiments, the second pre-curing can be specifically: curing the resin in the formed structure to more than 70%, that is, the curing degree of the resin after the second pre-curing is more than 70%, and the curing degree of the resin after the first pre-curing can be 70%, 75%, 80%, etc., so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. Preferably, the resin in the formed structure is cured to more than 80%, but not completely cured.
[0143] Alternatively, the second pre-curing may be specifically: placing the formed structure in a constant temperature environment of 170°C-185°C for 25min-35min to pre-cure the resin in the structure. Specifically, the formed structure may be placed in a constant temperature environment of 170°C, 175°C, 180°C or 185°C for 25min, 30min or 35min. Preferably, the formed structure is placed in a constant temperature environment of 180°C for 30min.
[0144] In the above-mentioned embodiments, the pre-curing in the S11 resin insulation layer processing step is hereinafter referred to as the third pre-curing. The third pre-curing may be specifically as follows: curing the resin insulation layer in the formed structure to above 70%-80%, that is, the curing degree is 70%-80%. Specifically, after the third pre-curing, the curing degree of the first resin insulation layer 11 may be 70%, 75%, 80%, etc., so as to harden the resin and improve the resin rigidity and mechanical impact resistance.
[0145] Alternatively, the third pre-curing may be specifically as follows: placing the formed structure in a constant temperature environment of 95°C-105°C for 25min-35min, and then placing it in a constant temperature environment of 170°C-185°C for 25min-35min. Specifically, the formed structure may be placed in a constant temperature environment of 95°C, 100°C or 105°C for 25min, 30min or 35min, and then placed in a constant temperature environment of 170°C, 180°C or 185°C for 25min, 30min or 35min. Preferably, the formed structure is placed in a constant temperature environment of 100°C for 30min, and then placed in a constant temperature environment of 180°C for 30min.
[0146] In the above-mentioned embodiments, the pre-curing in the process of processing the resin insulation layer in the step of making the intermediate circuit is hereinafter referred to as the fourth pre-curing. The fourth pre-curing can be specifically as follows: curing the resin insulation layer in the formed structure to more than 70%-80%, that is, the curing degree of the second resin insulation layer 13 after the fourth pre-curing is more than 70%. Specifically, the curing degree of the second resin insulation layer 13 after the fourth pre-curing can be 70%, 75%, 80%, etc., so as to harden the resin and improve the resin rigidity and mechanical impact resistance.
[0147] Alternatively, the fourth pre-curing may be specifically as follows: placing the formed structure in a constant temperature environment of 95°C-105°C for 25min-35min, and then placing it in a constant temperature environment of 170°C-185°C for 25min-35min. Specifically, the formed structure may be placed in a constant temperature environment of 95°C, 100°C or 105°C for 25min, 30min or 35min, and then placed in a constant temperature environment of 170°C, 180°C or 185°C for 25min, 30min or 35min. Preferably, the formed structure is placed in a constant temperature environment of 100°C for 30min, and then placed in a constant temperature environment of 180°C for 30min.
[0148] In an optional embodiment, the curing temperature of the first pre-curing is lower than the debonding temperature of the foaming film a of the first bonding material layer 2. If the debonding temperature of the foaming film a of the first bonding material layer 2 is 165°C-175°C, the first pre-curing temperature should be lower than 165°C-175°C. Specifically, the debonding temperature of the foaming film a of the first bonding material layer 2 can be 170°C. Preferably, the first pre-curing temperature is lower than the first debonding temperature by more than 10°C, or the first pre-curing temperature is lower than the first debonding temperature by 15°C-35°C. Specifically, the first pre-curing temperature can be lower than the first debonding temperature by 20°C or 30°C.
[0149] The curing temperature of the second pre-curing is at least 10°C lower than the debonding temperature of the foaming film a of the second bonding material layer 6, or the second pre-curing temperature is 15°C-25°C lower than the second debonding temperature. Preferably, the second pre-curing temperature can be 20°C lower than the second debonding temperature.
[0150] The debonding temperature of the foaming film a of the first bonding material layer 2 is lower than the debonding temperature of the foaming film a of the second bonding material layer 6, so that when the foaming film a of the first bonding material layer 2 is debonded, the foaming film a of the second bonding material layer 6 remains bonded to the first resin layer 5. The debonding temperature of the foaming film a of the first bonding material layer 2 may be 165°C-175°C, and preferably the debonding temperature of the foaming film a of the first bonding material layer 2 may be 170°C. The debonding temperature of the foaming film a of the second bonding material layer 6 may be 200°C-220°C, and preferably the debonding temperature of the foaming film a of the second bonding material layer 6 may be 210°C. Preferably, the debonding temperature of the foaming film a of the first bonding material layer 2 can be lower than the debonding temperature of the foaming film a of the second bonding material layer 6 by at least 15°C or 15°C-35°C. Specifically, the debonding temperature of the foaming film a of the first bonding material layer 2 can be lower than the debonding temperature of the foaming film a of the second bonding material layer 6 by 15°C, 20°C, 25°C, 30°C, or 35°C. Preferably, the debonding temperature of the foaming film a of the first bonding material layer 2 and the debonding temperature of the foaming film a of the second bonding material layer 6 differ by 30°C.
[0151] In addition, in a preferred embodiment, there is a protective film on the surface of the first resin layer 5. In the second temporary bonding step, the foaming film of the second bonding material layer 6 is bonded to the protective film of the first resin layer 5, so that the protective film can be torn off after debonding to prevent contamination.
[0152] The embodiment of the present invention also provides a temporary bonding structure, such as Figure 6 As shown, the temporary bonding structure includes: a substrate 1, a chip 4, a first bonding material layer 2, a first support plate 3, a first resin layer 5, a second bonding material layer 6 and a second support plate 7. The temporary bonding structure is specifically a structure formed after step S8. Specifically, the substrate 1 is provided with a receiving cavity 1a for receiving the chip 4, and the two surfaces of the substrate 1 are respectively a first bonding surface and a resin-filled surface. When the substrate 1 is placed horizontally, that is, when the thickness direction of the substrate 1 is along the vertical direction, the upper surface and the lower surface of the substrate 1 are respectively a resin-filled surface and a first bonding surface. The chip 4 is arranged in the receiving cavity 1a, and the electrode side of the chip 4 can be placed upwards, and the electrode side of the chip 4 can also be placed downwards. The first bonding material layer 2 is bonded to the first bonding surface, and the first support plate 3 is fixed to the side of the first bonding material layer 2 facing away from the substrate 1. As shown Fig.17 As shown, the first bonding material layer 2 may include a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the first bonding material layer 2 is bonded to the substrate 1. A first support plate 3 is fixed to the side of the first bonding material layer 2 facing away from the substrate 1, and the pressure-sensitive adhesive film c of the first bonding material layer 2 is bonded to the first support plate 3, that is, the first bonding material layer 2 is located between the first support plate 3 and the substrate 1.
[0153] The first resin layer 5 is located on the resin-filled surface of the substrate 1, and the side of the first resin layer 5 facing away from the substrate 1 is the second bonding surface. The resin-filled surface can be the upper surface of the substrate 1, and the resin fills the gaps between the circuits on the surface of the substrate 1 and the gaps around the chip 4. The second bonding material layer 6 is bonded to the second bonding surface, and the second bonding material layer 6 includes a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the second bonding material layer 6 is bonded to the first resin layer 5. A second supporting plate 7 is fixed to the side of the second bonding material layer 6 facing away from the first resin layer 5, and the pressure-sensitive adhesive film c of the second bonding material layer 6 is bonded to the second supporting plate 7. The second bonding surface is the upper surface of the first resin layer 5, and the second bonding material layer 6 is located between the second supporting plate 7 and the first resin layer 5, and the second supporting plate 7 is bonded to the side of the second bonding material layer 6 facing away from the first resin layer 5.
[0154] In the above temporary bonding structure, the foaming film of the first bonding material layer 2 is bonded to the first bonding surface of the substrate 1, and the foaming film a of the second bonding material layer 6 is bonded to the first resin layer 5, which can avoid contamination caused by the pressure-sensitive adhesive. In the process of debonding, in the first debonding step, it is only necessary to heat to the debonding temperature of the foaming film a of the first bonding material layer 2, and in the second debonding step, it is only necessary to heat to the debonding temperature of the foaming film a of the second bonding material layer 6, so that the foaming film is separated from the substrate 1 or the first resin layer 5. Compared with the pressure-sensitive adhesive film and the substrate 1 or the first resin layer 5, contamination caused by the pressure-sensitive adhesive can be avoided, and debonding is easier.
[0155] In the above-mentioned temporary bonding structure, the first support plate 3 and the second support plate 7 are used to provide support on both sides of the substrate 1 at the same time, so that in the steps of attaching the chip 4 and burying the first resin layer and the second resin layer, the first support plate 3 and / or the second support plate 7 support the substrate 1, thereby reducing the overall warping of the substrate 1 caused by the structural asymmetry during the manufacturing process of the embedded chip substrate, and ensuring that the substrate 1 is always in a low warping state during the entire manufacturing process of the embedded chip substrate.
[0156] In the above embodiment, the chip is preferably placed in the accommodating cavity, and the back of the chip 4 is bonded to the foam film of the first bonding material layer 2. The back of the chip 4 is the side of the chip 4 away from its pad, and the front of the chip 4 is the side with the pad. That is, the side of the chip away from the pad is bonded to the foam film a of the first bonding material layer 2. After the first debonding is completed, the temporary bonding glue residue generated during the debonding process of the foam film a is removed by cleaning. Cleaning includes water washing, ultrasonic water washing, and debonding in a debonding tank to effectively remove the temporary bonding glue residue on the surface of the substrate and the temporary bonding glue residue on the back of the chip. If the chip 4 has a side with a pad bonded to the foam film of the first bonding material layer 2, it is impossible to use a debonding tank for debonding, and more stringent cleaning is required, and the cleaning process is more complicated. Therefore, it is preferred that the back of the chip is bonded to the foam film a of the first bonding material layer 2.
[0157] Furthermore, the first support plate 3 can be a double-sided copper-clad plate, a metal plate, a glass plate or a ceramic plate, and each of the above types of plates has high rigidity. Similarly, the second support plate 7 can also be a double-sided copper-clad plate, a metal plate, a glass plate or a ceramic plate, and of course other types of plates can also be selected, which is not limited here.
[0158] The thickness of the first support plate 3 may be greater than or equal to 0.2 mm, specifically, the thickness of the first support plate 3 may be 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, etc. Further, the thickness of the first support plate 3 may be greater than or equal to 0.5 mm, such as 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, etc., so that the strength of the first support plate 3 can be ensured to prevent the substrate 1 from warping during processing.
[0159] The thickness of the second support plate 7 may be greater than or equal to 0.2 mm, specifically, the thickness of the second support plate 7 may be 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, etc. Further, the thickness of the second support plate 7 may be greater than or equal to 0.5 mm, such as 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, etc., so that the strength of the second support plate 7 can be ensured to prevent the substrate 1 from warping during processing.
[0160] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.
[0161] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for manufacturing an embedded chip substrate, characterized in that: Includes steps: A substrate window is provided, wherein a cavity for accommodating the chip is provided on the substrate, and two surfaces of the substrate are respectively a first bonding surface and a resin embedding surface; A first temporary bonding, bonding a first bonding material layer to the first bonding surface, wherein the first bonding material layer comprises a foaming film, a support film and a pressure-sensitive adhesive film stacked in sequence, and the foaming film of the first bonding material layer is bonded to the substrate, and a first support plate is fixed to a side of the first bonding material layer away from the substrate; Attaching the chip, placing the chip in the accommodating cavity; A first pressing and embedding resin, wherein the embedding resin is pressed and embedded on the embedding resin surface of the substrate to form a first resin layer, wherein a side of the first resin layer facing away from the substrate is a second bonding surface; Second temporary bonding, bonding a second bonding material layer to the second bonding surface, wherein the second bonding material layer comprises a foaming film, a support film and a pressure-sensitive adhesive film stacked in sequence, and the foaming film of the second bonding material layer is bonded to the first resin layer, and a second support plate is fixed to a side of the second bonding material layer away from the first resin layer, and performing a first pre-curing; A first debonding step is to debond the foaming film and the first bonding surface of the first bonding material layer to remove the first bonding material layer and the first support plate; Secondary pressing and embedding resin, pressing and embedding resin on the first bonding surface of the substrate to form a second resin layer, and performing a second pre-curing; second debonding, debonding the foamed film of the second bonding material layer from the first resin layer to remove the second bonding material layer and the second support plate; Blind hole processing, opening blind holes on the upper and lower surfaces of the structure formed in the previous step; Circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step; Resin insulation layer processing, in which a resin insulation layer is provided on both the upper surface and the lower surface of the structure formed in the previous step, and pre-cured; To make an intermediate circuit, repeat the steps of blind hole processing, circuit production and resin insulation layer processing N times, N ≥ 0, to form an N-layer intermediate circuit, and no pre-curing is performed in the N-th resin insulation layer processing step, and pre-curing is performed after copper foil is pressed on the surface of the resin insulation layer formed in the N-th resin insulation layer processing step, so that the resin insulation layer in the formed structure is cured to more than 50%; Curing: the structure formed in the previous step is placed in a laminator, clamped by a mirror steel plate, under a preset vacuum degree and a preset pressure, so that the resin in the structure is cured to more than 90%; Manufacturing the outer layer circuit, performing blind hole processing and circuit manufacturing steps on the cured structure to form the outer layer circuit; Making a solder resist layer, making a solder resist layer on the surface of the outer layer circuit; A coating is applied on the surface of the structure formed after the solder resist layer is made.
2. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: After the first debonding, the steps further include: first cleaning, cleaning the first bonding surface; and / or, After the second debonding, the method further includes a second cleaning step of cleaning the second bonding surface.
3. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The first pre-curing is specifically: curing the resin in the structure formed in this step to more than 50%; or, the first pre-curing is specifically: placing the structure formed in this step in a constant temperature environment of 130°C-150°C for 30min-60min to pre-cure the resin in the structure.
4. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The second pre-curing is specifically: curing the resin in the structure formed in this step to a degree of curing of more than 80%; or, the second pre-curing is specifically: placing the structure formed in this step in a constant temperature environment of 170°C-185°C for 25min-35min to pre-cure the resin in the structure.
5. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The pre-curing in the resin insulation layer processing step is specifically: curing the resin insulation layer in the structure to a degree of 70%-80%; or, the pre-curing in the resin insulation layer processing step is specifically: placing the formed structure in a constant temperature environment of 95°C-105°C for 25min-35min, and then placing it in a constant temperature environment of 170°C-185°C for 25min-35min.
6. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The raw materials used in the first pressing and filling resin step, the second pressing and filling resin step and the insulating layer processing step are all ABF resin sheets, and the ABF resin sheet includes an ABF layer, an OPP film attached to the first side of the ABF layer, and a PET film attached to the second side of the ABF layer.
7. The method for manufacturing an embedded chip substrate according to claim 6, characterized in that: The first resin embedding step is specifically as follows: removing the OPP film of the ABF resin sheet, and laminating the first side of the ABF resin sheet on the resin embedding surface of the substrate to form a first resin layer, and performing a first pre-curing so that the resin in the structure formed in this step is cured to more than 50%, and the side of the first resin layer away from the substrate is the second bonding surface and retains the PET film; and / or, The second pressing and filling resin step is specifically to remove the OPP film of the ABF resin sheet, and press the first side of the ABF resin sheet onto the first bonding surface of the substrate to form a second resin layer, and perform a second pre-curing to cure the resin in the structure formed in this step to more than 70%, and the second resin layer retains the PET film.
8. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The curing temperature of the first pre-curing is lower than the debonding temperature of the first bonding material layer; or, The debonding temperature of the first bonding material layer is lower than the debonding temperature of the second bonding material layer.
9. A temporary bonding structure, characterized in that: include: A substrate, wherein the substrate is provided with a receiving cavity for receiving the chip, and two surfaces of the substrate are respectively a first bonding surface and a resin embedding surface; A chip, wherein the chip is disposed in the accommodating cavity; A first bonding material layer and a first supporting plate, wherein the first bonding material layer is bonded to the first bonding surface, the first bonding material layer comprises a foaming film, a supporting film and a pressure-sensitive adhesive film stacked in sequence, the foaming film of the first bonding material layer is bonded to the substrate, and the first supporting plate is bonded to the pressure-sensitive adhesive film of the first bonding material layer; A first resin layer, the first resin layer is located on the buried resin surface of the substrate, and a side of the first resin layer facing away from the substrate is a second bonding surface; A second bonding material layer and a second supporting plate, the second bonding material layer is bonded to the second bonding surface, the second bonding material layer comprises a foaming film, a supporting film and a pressure-sensitive adhesive film stacked in sequence, the foaming film of the second bonding material layer is bonded to the first resin layer, and the second supporting plate is bonded to the pressure-sensitive adhesive film of the first bonding material layer.
10. The method for manufacturing an embedded chip substrate according to any one of claims 1 to 8 or the temporary bonding structure according to claim 9, characterized in that: The back side of the chip is bonded to the foaming film of the first bonding material layer.
11. The method for manufacturing an embedded chip substrate according to any one of claims 1 to 8 or the temporary bonding structure according to claim 9, characterized in that: The first support plate and / or the second support plate is a double-sided copper-clad plate, a metal plate, a glass plate or a ceramic plate; and / or the thickness of the first support plate and / or the second support plate is greater than 0.2 mm.
Citation Information
Patent Citations
Improved fanout panel level three-dimensional semiconductor chip package process
CN104103526A
Packaging method
CN114792632A
Manufacturing method and structure of packaging substrate
CN115939101A
Method and device for manufacturing semiconductor package
JP2011243801A
Semiconductor process sheet