Superlattice epitaxial structure with variable lattice parameter differences

By adopting superlattice epitaxial structure and alternating material layers on the silicon substrate, the lattice mismatch problem is solved, the performance and operating voltage of the device are improved, and the leakage current is reduced.

CN118943169APending Publication Date: 2024-11-12INFINEON TECH CANADA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410556197.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-05-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When growing wider bandgap semiconductor materials such as GaN on silicon substrates, there is significant lattice mismatch, resulting in defects and dislocations, and reducing device performance.

Method used

Using superlattice epitaxial structure, the mismatch is further biased by alternating the differences in lattice parameters by alternating the strain tolerance, reducing mismatch dislocations, and further biasing mismatch by changing the percentage of composition in the layer sequence. Dislocations enable the spiral dislocations that move upward during epitaxial growth to terminate, thereby improving the insulation of the structure.

Benefits of technology

A thinner superlattice structure and higher operating voltage are achieved, reducing leakage current from the active layer to the substrate and improving device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943169A_ABST
    Figure CN118943169A_ABST
Patent Text Reader

Abstract

A superlattice epitaxial structure epitaxially grown on a substrate. The superlattice epitaxial structure includes epitaxial layers constituting a plurality of layer sequences. Each of the plurality of layer sequences includes a corresponding lower layer and a corresponding upper layer epitaxially grown on the corresponding lower layer. The lattice parameter of the epitaxial layer is alternately lower and higher (or higher and lower) when moved upward through the superlattice epitaxial structure. The difference in lattice parameters in adjacent lower and higher epitaxial layers may also vary with upward movement through the epitaxial structure. Thus, by varying the difference between lattice parameters, the strain withstood at that level can be designed with the effect of increasing the resistance seen vertically through the superlattice epitaxial structure, allowing the structure to be thinner and / or operate at higher voltages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of power transistors, and more particularly, to a superlattice epitaxial stack for forming a power transistor. Background Art

[0002] Electronic circuits often include transistors, which act as electronic switches that regulate or control the flow of current in part of the circuit. One type of transistor is a field effect transistor, in which a voltage is applied to a gate terminal to turn the transistor on and off. A semiconductor channel region is arranged between a drain terminal and a source terminal. When the transistor is turned on, current flows through the semiconductor channel region between the source terminal and the drain terminal. When the transistor is turned off, less or no current flows through the semiconductor channel region between the source terminal and the drain terminal. The gate terminal is arranged on the semiconductor channel region between the source terminal and the drain terminal. The voltage on the gate terminal produces a field that affects whether the semiconductor channel region conducts current, hence the name "field effect transistor".

[0003] Silicon is traditionally used to make transistors. However, semiconductor materials with wider band gaps can be used to make transistors that conduct higher power and operate at higher efficiency than silicon transistors. Silicon carbide (SiC), aluminum nitride (AlN), zinc oxide (ZnO), and gallium nitride (GaN) are examples of wide band gap semiconductor materials that can be used in power electronics. However, it is not feasible to use substrates of these materials because they are expensive and more difficult to manufacture than silicon substrates. Therefore, wide band gap semiconductor materials are usually grown epitaxially on silicon substrates to facilitate high power electronics, taking advantage of the manufacturability and availability of silicon substrates combined with the wide band gap of the epitaxially grown material.

[0004] However, each semiconductor material has a crystal structure with a certain distance between repeating lattice points. This characteristic distance in a semiconductor crystal is often referred to as a "lattice constant" or "lattice parameter." Because the distance changes as the crystal structure expands and contracts with temperature, the term "lattice parameter" is used more frequently herein to avoid confusion in the fact that the lattice "constant" of a given semiconductor material can indeed change with temperature. However, at all operating temperatures, the lattice parameter of silicon can be completely different from the lattice parameter of a wider bandgap semiconductor material.

[0005] For example, when growing GaN on a silicon substrate, there is a significant lattice mismatch between the two materials, which can lead to defects and dislocations in the GaN layer. These defects can degrade the performance of GaN-based devices, such as high electron mobility transistors (HEMTs) and light-emitting diodes (LEDs). To address this problem, superlattice structures are often used as buffer layers between the silicon substrate and the GaN layer. Superlattice buffer layers consist of alternating layers of two different materials with different band gaps, which can be used to overcome the lattice mismatch between the two materials, resulting in a more structurally stable device.

[0006] The subject matter claimed herein is not limited to embodiments that solve any disadvantages or that operate only in environments such as described above. Rather, this background is merely provided to illustrate one exemplary technology area in which some embodiments described herein may be practiced. Summary of the invention

[0007] This Summary is provided to introduce some concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.

[0008] Embodiments described herein relate to a superlattice epitaxial structure epitaxially grown on a substrate. The superlattice epitaxial structure includes epitaxial layers constituting a plurality of layer sequences. Each of the plurality of layer sequences includes a corresponding lower layer and a corresponding upper layer epitaxially grown on the corresponding lower layer. The lattice parameters of the lower epitaxial layers are alternately lower and higher (or higher and lower) when moving upward through the superlattice epitaxial structure. The difference in lattice parameters in the adjacent lower and higher layers can also change as the epitaxial structure is moved upward. Therefore, by changing the difference between the lattice parameters, the strain tolerated at this level can be designed. For example, the engineering can be such that misfit dislocations are generated further downward in the superlattice structure compared to what occurs when the difference in lattice parameters is kept relatively the same by moving upward through the superlattice epitaxial structure. These misfit dislocations typically end in screw dislocations that can move upwardly during epitaxial growth. Since screw dislocations can be conductive, this has the effect of allowing the upper portion of the superlattice structure to act more as an insulator, thereby allowing the superlattice structure to be thinner and / or allowing an increase in operating voltage.

[0009] By way of example only, there may be a repeating pattern of two different semiconductor materials where the composition percentage of one (or both) of the two different layers may be allowed to change as one moves up through the superepitaxial structure. For example, there may be a repeating pattern of AlN and AlGaN where the percentage of the Al composition of the AlGaN layer decreases (and thus the Ga composition increases) for each successive AlGaN layer. By way of example only, the composition may move in a linear fashion from 100% AlN to 100% GaN moving up through the superepitaxial structure. Doing so would actually have the effect of biasing the misfit dislocations further down in the superepitaxial structure.

[0010] Additional features and advantages will be set forth in the following description, and in part will be apparent from the description, or may be learned by practicing the teachings herein. The features and advantages of the present invention may be realized and obtained by the means and combinations particularly pointed out in the appended claims. The features of the present invention will become more apparent from the following description and the appended claims, or may be learned by practicing the present invention as described below. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to describe the manner in which the above-recited and other advantages and features can be obtained, a more particular description of the subject matter briefly described above will be rendered by reference to specific embodiments that are illustrated in the accompanying drawings. Understanding that these drawings depict only typical embodiments and are therefore not to be considered limiting of scope, the embodiments will be described and explained with additional specificity and detail through the use of the accompanying drawings, in which:

[0012] Figure 1 A crystal unit cell view of a gallium nitride (GaN) crystal unit cell superimposed on a silicon crystal unit cell is shown, each crystal unit cell being oriented so that the hexagonal closed-packed array of atoms defining each unit cell faces the viewer;

[0013] Figure 2A An example structure is shown in which an upper semiconductor layer is deposited (eg, by epitaxial growth) on a lower semiconductor layer.

[0014] Figure 2B It shows that the deposition Figure 2A The lower semiconductor layer Figure 2A Side view of the upper semiconductor layer.

[0015] Figure 3A and Figure 3B Respectively similar to Figure 2A and Figure 2B , except to show that the opposite effect may also occur when a layer of higher lattice parameter semiconductor material is grown on a layer of lower lattice parameter semiconductor material.

[0016] Figure 3B A side view is shown, which illustrates that these compressive forces tend to cause the structure to convex.

[0017] Figure 4 A side view of an example structure is shown in which an upper semiconductor layer of lower lattice parameter is deposited on a lower semiconductor layer of higher lattice parameter.

[0018] Figure 5 Shown is an actual transmission electron microscope (TEM) image of a GaN layer grown on an AlN layer grown on a Si wafer.

[0019] Figure 6A time course graph of wafer bow as the wafer is processed to have multiple epitaxial layers is shown.

[0020] Fig. 7A A side view of a single layer sequence comprising a lower semiconductor layer and an upper semiconductor layer is shown.

[0021] Figure 7B : is a composition diagram in which the vertical position in the superlattice epitaxial structure is represented on the vertical axis, and the percentage composition of Al in the corresponding layer at the vertical position is represented on the horizontal axis.

[0022] Fig. 8A and Figure 8B An example superepitaxial structure is shown wherein a lower semiconductor layer is comprised of AlGaN wherein the Al percentage increases linearly from 0% to 100% moving up through the superepitaxial structure, and wherein an upper semiconductor layer is comprised of AlGaN wherein the Al percentage decreases linearly from 100% to 0% moving up through the superepitaxial structure; and

[0023] Fig.9A and Fig. 9B An example superepitaxial structure is shown in which a lower semiconductor layer has M% AlGaN (where M is 28 in this specific example), and in which the Al percentage in an upper semiconductor layer composed of AlGaN decreases linearly from 100% to 5% in an exponential manner, moving up through the superepitaxial structure. DETAILED DESCRIPTION

[0024] Embodiments described herein relate to a superlattice epitaxial structure epitaxially grown on a substrate. The superlattice epitaxial structure includes epitaxial layers constituting a plurality of layer sequences. Each of the plurality of layer sequences includes a corresponding lower layer and a corresponding upper layer epitaxially grown on the corresponding lower layer. The lattice parameters of the lower epitaxial layers are alternately lower and higher (or higher and lower) when moving upward through the superlattice epitaxial structure. The difference in lattice parameters in the adjacent lower and higher layers can also change as the epitaxial structure is moved upward. Therefore, by changing the difference between the lattice parameters, the strain tolerated at this level can be designed. For example, the engineering can be such that misfit dislocations are generated further downward in the superlattice structure compared to what occurs when the difference in lattice parameters is kept relatively the same by moving upward through the superlattice epitaxial structure. These misfit dislocations typically end in screw dislocations that can move upwardly during epitaxial growth. Since screw dislocations can be conductive, this has the effect of allowing the upper portion of the superlattice structure to act more as an insulator, thereby allowing the superlattice structure to be thinner and / or allowing an increase in operating voltage.

[0025] By way of example only, there may be a repeating pattern of two different semiconductor materials where the composition percentage of one (or both) of the two different layers may be allowed to change as one moves up through the superepitaxial structure. For example, there may be a repeating pattern of AlN and AlGaN where the percentage of the Al composition of the AlGaN layer decreases (and thus the Ga composition increases) for each successive AlGaN layer. By way of example only, the composition may move in a linear fashion from 100% AlN to 100% GaN moving up through the superepitaxial structure. Doing so would actually have the effect of biasing the misfit dislocations further down in the superepitaxial structure.

[0026] Figure 1 A crystal unit cell view 100 of a gallium nitride (GaN) crystal unit cell 110A superimposed on a silicon crystal unit cell 110B is shown, with each crystal unit cell oriented so that the hexagonal closed-packed atomic array defining each cell faces the viewer. If the GaN layer is grown directly on <111> On a Si layer with a plane orientation, each layer will be formed by units in a hexagonal closed packing array at the interface between the two layers. <111> In the Si orientation, a silicon crystal has a hexagonal structure with a lattice parameter of 3.840 angstroms on each hexagonal side. On the other hand, a GaN crystal has a hexagonal structure with a lattice parameter of 3.189 angstroms when oriented along a hexagonal closed packing array. This lattice parameter difference is extreme. Therefore, it is not standard practice to grow GaN layers directly on Si substrates due to the extreme lattice parameter mismatch. However, a discussion of what would happen if a GaN layer were grown directly on a Si substrate would help understand the stress caused by the lattice mismatch between the two different semiconductor materials.

[0027] Each point in the lattice structure is an atom of the crystal, and each link between the points is a bond between adjacent atoms in the crystal. If GaN does grow on Si, then each Ga or N atom in the GaN layer will bond to a corresponding Si atom in the Si layer. This will cause the GaN layer to experience a tensile stress with a corresponding compressive stress on the Si layer. Therefore, the Ga or N atom at point 111A will bond to the Si atom at point 111B. Similarly, the Ga or N atoms at points 112A to 116A will bond to the Si atoms at points 112B to 116B, respectively. Therefore, when one semiconductor material is grown on another semiconductor material in a hexagonal orientation, there will be strain and stress in the interface between the two semiconductor materials. This means that in the context of semiconductor manufacturing, when a semiconductor layer is deposited on another semiconductor layer, reference will now be made to FIG. 2A to FIG. 3B Give a description.

[0028] Figure 2AAn example structure 200 is shown in which an upper semiconductor layer 202 is deposited (e.g., by epitaxial growth) on a lower semiconductor layer 201. As an example, the lower semiconductor layer 201 can be an upper surface of a wafer (e.g., a silicon wafer), and the upper semiconductor layer 202 can be a wide bandgap semiconductor material layer epitaxially grown on the wafer.

[0029] The gate pattern of each of the upper semiconductor layer 202 and the lower semiconductor layer 201 represents a characteristic repeating pattern in each respective semiconductor material. The gate pattern of the upper semiconductor layer 202 shows a horizontal distance 212 between vertical lines, which represents the lattice parameter along the horizontal plane. On the other hand, the gate pattern of the lower semiconductor layer 201 has a larger horizontal distance 211 between vertical lines, indicating that the lower semiconductor layer 201 has a larger lattice parameter than the upper semiconductor layer 202. Molecules from one crystalline material will attempt to bond with molecules in another crystalline material. Therefore, this will cause the upper semiconductor layer 202 to have a tensile stress as shown by arrows 203A and 203B (and there will be corresponding compressive stress in the lower semiconductor layer 201).

[0030] Figure 2B FIG. 2 shows a side view of an upper semiconductor layer 202 deposited on a lower semiconductor layer 201. For example, if the lower semiconductor layer 201 is a silicon wafer substrate, then Figure 2B A side view of the wafer is shown. Figure 2B The tensile strain of the upper semiconductor layer will cause the entire wafer to be stretched in the deposition direction (e.g., in Figure 2B Since the silicon wafer is relatively thick compared to the epitaxial layer, the concave curvature will be very slight. As previously mentioned, the lower semiconductor layer 201 can be a silicon wafer, and the upper semiconductor layer 202 can be a wide bandgap semiconductor material layer epitaxially grown on the top surface of the wafer. However, when growing a crystalline material with a smaller lattice parameter on a crystalline material with a larger lattice parameter, the above-mentioned curvature can be applied. Figure 2A and Figure 2B Principle of description.

[0031] Figure 3A and Figure 3B Respectively similar to Figure 2A and Figure 2B , except to show that the opposite effect can also occur when a layer of a larger lattice parameter semiconductor material is grown on a layer of a smaller lattice parameter semiconductor material. For example, Figure 3AAn example structure 300 is shown in which an upper semiconductor layer 302 is grown on a lower semiconductor layer 301. Here, the lattice parameter of the higher semiconductor layer 302 (represented by distance 312) is greater than the lattice parameter of the lower semiconductor layer 301 (represented by distance 311). Therefore, when atoms in the corresponding lattices attempt to bond, the upper semiconductor layer 302 experiences compressive stress as shown by arrows 303A and 303B (and will experience corresponding tensile stress in the lower semiconductor layer 301). Figure 3B A side view is shown, which illustrates that these compressive forces tend to cause the structure to convex.

[0032] Therefore, as mentioned above FIG. 2A to FIG. 3B As shown, when semiconductor materials of different lattice parameters are joined by epitaxial growth, the wafer will bend due to the strain induced. In the case of epitaxial growth of many layers of different materials, each new layer will experience compressive or tensile stress, applying the corresponding tensile or compressive stress to the structure on which the new epitaxial layer is grown.

[0033] When a crystalline material is epitaxially grown on top of a crystalline material of a different lattice parameter, misfit dislocations will inevitably exist. For example, Figure 4 A side view of an example structure 400 is shown, in which an upper semiconductor layer 402 of smaller lattice parameter is deposited on a lower semiconductor layer 401 of larger lattice parameter. In this case, the atoms of the upper layer 402 will stretch to form bonds with corresponding atoms in the lower semiconductor layer 401, but only to a limit. At a certain point, the atoms in the upper semiconductor layer 402 (e.g., see point 420) will not form bonds with the atoms immediately below. Instead, neighboring atoms 421 and 422 of the upper semiconductor 402 will form bonds with atoms 411 and 412 immediately below. This results in a misfit dislocation 410. The misfit dislocation will continue laterally along the crystal until it is terminated by the edge of the material, or more frequently, by a screw dislocation that extends upward during growth.

[0034] The presence of misfit dislocations 410 promotes the creation of screw dislocations that extend upward in the material. Figure 5 An actual transmission electron microscope (TEM) image 500 of a GaN layer grown on an AlN layer grown on a Si wafer is shown. The darker areas represent dislocations caused by lattice mismatch. The horizontal channels are mismatch dislocations that propagate the vertical channels of screw dislocations. Since screw dislocations are more conductive, this makes the superlattice structure have less resistance in the vertical direction. This can cause undesirable leakage current from the active layer to the substrate, thereby compromising the performance of the transistor.

[0035] Furthermore, as each epitaxial layer is formed, the wafer will become more convex or more concave, depending on whether the new epitaxial layer is subject to tensile or compressive stress due to lattice parameter mismatch with the adjacent underlying layer. Figure 6A time course graph 600 of wafer curvature is shown as the wafer is processed to have multiple epitaxial layers. In this particular time course graph 600, both the temperature and the type of material being epitaxially grown have an effect on the curvature of the wafer. In this specific example, an AlN layer is epitaxially grown on a Si wafer during time period 601. Thereafter, during time period 602, a superlattice epitaxial structure is epitaxially grown on the AlN, which includes GaN and possibly AlN in various combinations. Thereafter, during time period 603, the wafer is cooled to normal ambient temperature.

[0036] As shown by line 611, during time period 601, the wafer becomes more steadily concave due to the lower lattice parameter of AlN compared to Si, and further due to the higher temperatures required to epitaxially grow AlN on Si. On the other hand, during time period 603, as shown by line 613, cooling of the wafer causes the convex wafer to become less convex to the point where the curvature is low enough so that the wafer is a suitably flat base to fabricate additional structures on the superlattice structure. The goal of time period 602 is to grow the superlattice structure with sufficient strain engineering so that at the end of time period 602, the wafer has sufficient curvature so that cooling (during time period 603) will produce a sufficiently flat wafer to form additional structures (such as active areas of a circuit) thereon.

[0037] Although lines 611 to 613 are shown as straight lines, the curvature of the wafer does not generally change linearly with time. However, lines 611 to 613 are merely used to illustrate the larger principle that a superlattice structure can be formed by strain engineering so that the wafer is sufficiently convex so that subsequent cooling will produce a relatively flat wafer. In order to bias the misfit dislocations so that they are generated more toward the lower portion of the superlattice epitaxial structure, line 612 should be a curve that drops more steeply at the beginning of time period 602 and has a gentler slope at the end of time period 602.

[0038] According to the principles described herein, superepitaxial structures are constructed so that the difference in lattice parameters of adjacent semiconductor layers changes as one moves up through the superepitaxial structure. This helps to make line 612 curve as it does, and thus tends to cause misfit dislocations to occur lower in the superepitaxial structure.

[0039] Fig. 7A and Figure 7B Specific examples are shown together in which a superepitaxial structure comprises a number of repeating layer sequences. Fig. 7A A side view of a single layer sequence 700A including a lower layer 701 and an upper layer 702 is shown. Fig. 7AThe layer sequence may be repeated N times, moving up through the superlattice epitaxial structure, where N is some positive integer. Thus, when the repeating layer sequence is stacked, the stack includes layers that alternate between lower layers 701 and upper layers 702. However, in each subsequently deposited layer sequence, the composition of one or both of the lower layers 701 or upper layers 702 may vary. If this is done for at least some of the layer sequences, this allows the lattice parameter difference (i.e., lattice mismatch) between the corresponding lower and upper layers to vary moving up through the layer sequence in the superlattice epitaxial structure.

[0040] Figure 7B is a composition diagram where the vertical position in the superlattice epitaxial structure is represented on the vertical axis, and the percentage composition of Al in the corresponding layer at that vertical position is represented on the horizontal axis. In this specific example, the composition of the lower layer 701 remains the same. Specifically, in this example, the composition of the lower layer 701 is 28% AlGaN. Therefore, this layer is 28% Al and 72% Ga. However, in this example, the upper layer 702 is AlGaN, but its Al content varies linearly from 100% to 0%. Therefore, in Figure 7B Moving vertically upward in FIG. 7 , 26 oscillations of the Al content between 28% (each corresponding to the lower layer 701 ) and some other value (each corresponding to the upper layer 702 ) are found.

[0041] exist Figure 7B In order to avoid the lines becoming too close together and difficult to read, there are only 26 such oscillations representing a 26-layer sequence. However, N is usually much larger (e.g., 93). Figure 7B The general principle is shown. That is, in the lowest layer sequence, the upper layer 702 is 100% AlN. However, in the highest layer sequence, the upper layer 702 is 100% GaN. More generally, through X% of the superlattice epitaxial structure, the composition of the upper semiconductor layer 702 is approximately (100-X)% AlN and X% GaN. Compared to having the upper semiconductor layer 702 have a constant composition for each layer sequence, this gradual change in the composition of the upper semiconductor layer 702 will cause misfit dislocations to accumulate further down in the superlattice epitaxial structure.

[0042] More broadly, the first composite material of each lower semiconductor layer 701 can be a composite material of AlN and GaN consisting of M% AlN (where M is a number between 0 and 100), and the second composite material of each upper semiconductor layer can also be a composite material of AlN and GaN containing N% AlN (where N is also a number between 0 and 100, but different from M).

[0043] However, the materials of the lower semiconductor layer 701 and the upper semiconductor layer 702 may be any semiconductor material. By way of example only, the first composite material for each lower semiconductor layer 701 may be a composite material of InAs and GaAs consisting of M% InAs (where M is a number between 0 and 100), and the second composite material for each upper semiconductor layer may also be a composite material of InAs and GaAs containing N% InAs (where N is also a number between 0 and 100, but different from M).

[0044] However, the semiconductor material of the lower semiconductor layer 701 can be any semiconductor material in which the first semiconductor material has M% of a specific component element and the second semiconductor material has the same composition but has N% of a specific component element. More generally, the lower semiconductor material and the upper semiconductor material do not even have to be made of the same composition. For example, one layer can be InGaN and the other layer can be AlGaN. As another example, one layer can be AlInGaN and the other layer can be AlGaN or InGaN. However, if the layers have the same composition but different percentages of component elements, manufacturing will be easier because only the element ratios need to be changed, which can usually be done with a single epitaxial deposition machine.

[0045] The more general principles described here are in no way limited to reference Fig. 7A and Figure 7B For example, in Fig. 7A , the lower layer 701 is described as 28% AlGaN, and the upper semiconductor layer 702 is described as AlGaN, but its Al content varies linearly from 100% to 0%. In other words, M is fixed at 28, and N is allowed to vary linearly from 100 to 0, moving up through the superlattice epitaxial structure. However, M can be fixed at any number, and / or N can vary linearly, but not across the entire range from 100 to 0. For example, N can vary linearly from a percentage less than 100 percent (e.g., 80 percent), and / or end the linear change at a percentage greater than 0 percent (e.g., 20 percent).

[0046] As described above, the composition percentage N of the upper semiconductor layer 702 is allowed to change, while the composition percentage M of the lower semiconductor layer 701 remains constant. Alternatively, the composition percentage N of the upper semiconductor layer 702 remains constant, while the composition percentage M of the lower semiconductor layer 701 may be allowed to change. Alternatively, both the composition percentage N of the upper semiconductor layer 702 and the composition percentage M of the lower semiconductor layer 701 are allowed to change.

[0047] Where changes are permitted, the composition percentages M and N may vary monotonically or non-monotonically. Monotonically varying means that the composition percentages either only increase moving up through the superlattice epitaxial structure, or only decrease moving up through the superlattice epitaxial structure. In addition, where changes are permitted, the composition percentages M and N may vary linearly or non-linearly. When both M and N are permitted to vary, they may both vary linearly, both vary non-linearly, or one may vary linearly and the other non-linearly.

[0048] Fig. 8A and Figure 8B An example super-epitaxial structure is shown, wherein the lower semiconductor layer 801 is composed of AlGaN, wherein the Al percentage increases linearly from 0% to 100%, moving up through the super-epitaxial structure. In addition, the upper semiconductor layer 802 is composed of AlGaN, wherein the Al percentage decreases linearly from 100% to 0%, moving up through the super-epitaxial structure.

[0049] Fig.9A and Fig. 9B An example superepitaxial structure is shown in which a lower semiconductor layer 701 has M% AlGaN (where M is 28 in this specific example), and in which the Al percentage in an upper semiconductor layer 702 composed of AlGaN decreases exponentially from 100% to 5%, moving upward through the superepitaxial structure.

[0050] Each of these examples will result in a further downward misfit dislocation in the superlattice epitaxial structure compared to the case where the composition percentages of the upper and lower semiconductor layers remain constant. However, this can also be achieved in many cases where the difference in lattice parameters of the upper and lower semiconductor layers is allowed to change as one moves upward through the superlattice epitaxial structure. In addition, in the present specification, one layer sequence is different from another layer sequence in the composition and / or material of one or both of the lower semiconductor layer or the upper semiconductor layer. However, the generation of misfit dislocations can also be achieved by changing the thickness of one or both of the upper or lower semiconductor layers in the continuous layer sequence. Finally, although the principles described here are described in the context of each layer sequence having two component layers, the principles described here can also be applied to the case where there are more than two component layers in the layer sequence. However, even in this case, one of the component layers can be considered to be a lower semiconductor layer adjacent to the upper semiconductor layer.

[0051] Thus, a superepitaxial structure has been described that allows flexibility in changing the sequence of layers moving up through the superepitaxial structure so that misfit dislocations are further down in the superepitaxial structure than if the sequence of layers were not changed. Thus, the resistance of the superepitaxial structure in a direction perpendicular to the epitaxial growth direction can be increased, thereby reducing current leakage from the active region to the substrate. This allows the superepitaxial structure to be thinner, and / or facilitates the growth of high-power electronic devices that can operate at higher voltages.

[0052] Text support part

[0053] Item 1. A superlattice epitaxial structure epitaxially grown on a substrate, the superlattice epitaxial structure comprising a plurality of epitaxial layers consisting of a plurality of layer sequences, each of the plurality of layer sequences comprising a corresponding lower layer and a corresponding upper layer epitaxially grown on the corresponding lower layer, wherein for a first layer sequence in the plurality of layer sequences, the lower layer has a lattice parameter, the lattice parameter having a magnitude polarity compared to the substrate and higher layers of the first layer sequence, wherein for additional layer sequences in the plurality of layer sequences, the lower layer of the corresponding layer sequence has a magnitude polarity compared to higher layers of the previous layer sequence and to higher layers of the corresponding layer sequence, and the difference between the lattice parameters of the lower and higher layers of one layer sequence is different from the lattice parameters of the lower and higher layers of another layer sequence.

[0054] Clause 2. The superepitaxial structure of Clause 1, wherein for each of at least some of the plurality of layer sequences, the underlying layer has a different thickness.

[0055] Clause 3. The superepitaxial structure of clause 1, wherein for each of at least some of the plurality of layer sequences, the higher layers have a different thickness.

[0056] Item 4. The superlattice epitaxial structure according to Item 1, wherein the lower layer for each of the plurality of layer sequences is composed of the first composite material for each of the plurality of layer sequences, and the upper layer for each of the plurality of layer sequences is composed of the second composite material for each of the plurality of layer sequences.

[0057] Item 5. According to the superlattice epitaxial structure of Item 4, the first composite material used for each lower layer is a composite material of AlN and GaN having a composition of M% AlN (where M is a number between 0 and 100), and the second composite material used for each higher layer is a composite material of AlN and GaN having a composition of N% AlN (where N is a number between 0 and 100), wherein for each of a plurality of layer sequences, M and N are different for each of at least some of the plurality of layer sequences.

[0058] Item 6. According to the superlattice epitaxial structure of Item 4, the first composite material used for each lower layer is a composite material of InN and GaN having a composition of M% InN (where M is a number between 0 and 100), and the second composite material used for each higher layer is a composite material of InN and GaN having a composition of N% InN (where N is a number between 0 and 100), wherein M and N are different for each of at least some of the multiple layer sequences.

[0059] Clause 7. The superepitaxial structure of Clause 4, wherein for each successive underlying layer in the plurality of layer sequences, the composition percentage of the first composite material varies.

[0060] Clause 8. The superepitaxial structure of Clause 7, wherein the composition percentage of the first component material varies linearly for each successive underlying layer in the plurality of layer sequences.

[0061] Clause 9. The superepitaxial structure of clause 7, wherein for each successive underlying layer in the plurality of layer sequences, the composition percentage of the first component material varies non-linearly.

[0062] Clause 10. The superepitaxial structure of Clause 7, wherein for each successive lower layer in the plurality of layer sequences, the composition percentage of the first composite material varies monotonically.

[0063] Clause 11. The superepitaxial structure of Clause 7, wherein the composition percentage of the second composite material varies for each successive underlying layer in the plurality of layer sequences.

[0064] Clause 12. The superepitaxial structure of clause 11, wherein the composition percentage of the second component material changes linearly for each successively higher layer in the plurality of layer sequences.

[0065] Clause 13. The superepitaxial structure of clause 11, wherein the composition percentage of the second component material varies non-linearly for each successively higher layer in the plurality of layer sequences.

[0066] Clause 14. The superepitaxial structure of Clause 11, wherein the composition percentage of the second composite material changes monotonically for each successively higher layer in the plurality of layer sequences.

[0067] Clause 15. The superepitaxial structure of Clause 4, wherein the composition percentage of the second composite material varies for each successive underlying layer in the plurality of layer sequences.

[0068] Clause 16. The superepitaxial structure of Clause 15, wherein the composition percentage of the second component material changes linearly for each successively higher layer in the plurality of layer sequences.

[0069] Clause 17. The superepitaxial structure of clause 15, wherein the composition percentage of the second component material varies non-linearly for each successively higher layer in the plurality of layer sequences.

[0070] Clause 18. The superepitaxial structure of Clause 15, wherein the composition percentage of the second composite material changes monotonically for each successively higher layer in the plurality of layer sequences.

[0071] Although the subject matter has been described in language specific to structural features and / or methodological actions, it should be understood that the subject matter defined in the appended claims is not necessarily limited to the features or actions described above, or the order of the actions described above. Instead, the described features and actions are disclosed as example forms of implementing the claims.

[0072] The present disclosure may be implemented in other specific forms without departing from its essential features. The described embodiments are considered in all respects to be illustrative rather than restrictive. All changes within the equivalent meaning and range of the claims are included within their scope.

[0073] When introducing elements in the appended claims, the articles "a," "an," "the," and "said" are intended to mean that there are one or more of the elements. The terms "comprising," "including," and "having" are intended to be inclusive and mean that there may be additional elements other than the listed elements.

Claims

1. A superlattice epitaxial structure epitaxially grown on a substrate, the superlattice epitaxial structure comprising a plurality of epitaxial layers consisting of a plurality of layer sequences, each of the plurality of layer sequences comprising a corresponding lower layer and a corresponding upper layer epitaxially grown on the corresponding lower layer, wherein for a first layer sequence of the plurality of layer sequences, the lower layers have a lattice parameter which has an amplitude polarity compared to the substrate and to higher layers of the first layer sequence, wherein for an additional layer sequence of the plurality of layer sequences, the lower layers of the corresponding layer sequence have the amplitude polarity compared to the higher layers of the preceding layer sequence and compared to the higher layers of the corresponding layer sequence, The difference between the lattice parameters of the lower and higher layers of one layer sequence is different from the lattice parameters of the lower and higher layers of another layer sequence. 2 . The superlattice epitaxial structure of claim 1 , wherein the lower layer has a different thickness for each of at least some of the plurality of layer sequences. 3 . The superepitaxial structure of claim 1 , wherein for each of at least some of the plurality of layer sequences, the higher layer has a different thickness.

4. In the superlattice epitaxial structure according to claim 1, the lower layer for each of the multiple layer sequences is composed of a first composite material for each of the multiple layer sequences, and the higher layer for each of the multiple layer sequences is composed of a second composite material for each of the multiple layer sequences.

5. The superlattice epitaxial structure according to claim 4, wherein the first composite material used for each lower layer is a composite material of AlN and GaN having a composition of M% AlN (wherein M is a number between 0 and 100), and the second composite material used for each higher layer is a composite material of AlN and GaN having a composition of N% AlN (wherein N is a number between 0 and 100), wherein for each of a plurality of layer sequences, M and N are different for each of at least some of the plurality of layer sequences.

6. In the superlattice epitaxial structure according to claim 4, the first composite material used for each lower layer is a composite material of InN and GaN having a composition of M% InN (wherein M is a number between 0 and 100), and the second composite material used for each higher layer is a composite material of InN and GaN having a composition of N% InN (wherein N is a number between 0 and 100), wherein M and N are different for each of at least some of the multiple layer sequences.

7. The super-epitaxial structure of claim 4, wherein the composition percentage of the first composite material varies for each successive lower layer in the plurality of layer sequences. 8 . The superlattice epitaxial structure of claim 7 , wherein the composition percentage of the first component material varies linearly for each successive lower layer in the plurality of layer sequences.

9. The superlattice epitaxial structure of claim 7, wherein for each successive lower layer in the plurality of layer sequences, the composition percentage of the first component material varies nonlinearly.

10. The super-epitaxial structure of claim 7, wherein for each successive lower layer in the plurality of layer sequences, the composition percentage of the first composite material varies monotonically.

11. The superepitaxial structure of claim 7, wherein the composition percentage of the second composite material varies for each successive lower layer in the plurality of layer sequences.

12. The superlattice epitaxial structure of claim 11, wherein the composition percentage of the second component material changes linearly for each successively higher layer in the plurality of layer sequences.

13. The superlattice epitaxial structure of claim 11, wherein the composition percentage of the second component material varies non-linearly for each successively higher layer in the plurality of layer sequences.

14. The superepitaxial structure of claim 11, wherein the composition percentage of the second composite material varies monotonically for each successively higher layer in the plurality of layer sequences.

15. The superepitaxial structure of claim 4, wherein the composition percentage of the second composite material varies for each successive lower layer in the plurality of layer sequences.

16. The superlattice epitaxial structure of claim 15, wherein the composition percentage of the second component material changes linearly for each successively higher layer in the plurality of layer sequences.

17. The superlattice epitaxial structure of claim 15, wherein the composition percentage of the second component material varies non-linearly for each successively higher layer in the plurality of layer sequences.

18. The superepitaxial structure of claim 15, wherein the composition percentage of the second composite material varies monotonically for each successively higher layer in the plurality of layer sequences.