Infrared photoelectric detector based on graphene nanobelt and preparation method thereof

By constructing a vertical heterojunction structure of graphene nanoribbon/hafnium oxide/gallium arsenide, the problem of high dark current of graphene photodetectors is solved, high response and low power consumption in the near-infrared band are achieved, and photodetection is improved performance of the device.

CN118943228APending Publication Date: 2024-11-12SHANDONG UNIV SHENZHEN RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410937429.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing graphene photodetectors have small light response and poor light absorption efficiency due to excessive dark current, which limits their application in infrared detectors.

Method used

Construct graphene nanoband/hafnium oxide/gallium arsenide vertical heterojunction structure, introduce electron band gap through quantum confined domain effect, control carrier concentration, reduce dark current, and achieve high in the near-infrared band by reasonably building device structure Responsive and low dark current.

Benefits of technology

It realizes stable near-infrared detection capability and low power consumption under voltage-free conditions, and improves the response and sensitivity of the photodetector.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943228A_ABST
    Figure CN118943228A_ABST
Patent Text Reader

Abstract

The invention relates to an infrared photoelectric detector based on a graphene nanobelt and a preparation method of the infrared photoelectric detector. The infrared photoelectric detector sequentially comprises an n-type gallium arsenide substrate, an n-type material contact electrode layer, a hafnium oxide layer, a p-type graphene nanobelt layer and a p-type material contact electrode layer from bottom to top. The photoelectric detector obtained by the preparation method provided by the invention has strong response to short-wave infrared light, and the device still has stable infrared light detection capability under the condition of not applying voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a graphene nanoribbon-based infrared photoelectric detector and a preparation method thereof, and belongs to the technical field of semiconductor optoelectronics. Background Art

[0002] Infrared photodetectors have been effectively used in industry, science, military and daily life. Currently, commercial infrared detectors are mainly made of narrow bandgap materials such as Si, Ge, GaAs and HgCdTe. However, the narrow bandgap of these materials makes the infrared detectors have high dark current, resulting in high power consumption, which restricts their development in the new generation of infrared detectors.

[0003] Two-dimensional materials have been widely studied in the field of optoelectronic devices due to their large specific surface area, surface without dangling bonds, and excellent optoelectronic properties. Graphene, as a typical two-dimensional material, has extremely high carrier mobility at room temperature (tens of times higher than that of Si materials), fast photoresponse and ultra-wideband light absorption, and is considered to be a promising candidate for optoelectronic materials. However, although the zero-bandgap band structure of graphene provides an extremely wide absorption wavelength range, it also leads to extremely low light absorption efficiency; at the same time, the ultra-high carrier concentration in graphene leads to extremely high dark current of graphene-based infrared detectors, resulting in low on / off ratio and high signal noise of the device. How to reduce the dark current to a lower level and maintain excellent infrared light detection capability is the main obstacle that needs to be solved in the practical application of graphene photodetectors. Graphene nanoribbons cleverly introduce a considerable electronic band gap into graphene through the quantum confinement effect. The existence of the band gap makes the carrier concentration of graphene nanoribbons controllable while still retaining the high carrier mobility of the original graphene. Therefore, by constructing a graphene nanoribbon / hafnium oxide / gallium arsenide vertical heterojunction, the dark current can be effectively reduced and a low-power and high-response infrared photodetector can be realized. Summary of the invention

[0004] In view of the problems existing in this field, the present invention aims to solve the problems of existing graphene photodetectors having too high dark current, resulting in small light response and poor light absorption efficiency.

[0005] To solve the above problems, the present invention aims to construct a graphene nanoribbon / hafnium oxide / gallium arsenide vertical heterojunction infrared photodetector. The technical problem to be solved is to use graphene nanoribbons and reasonably construct the device structure so that it has ultra-high response and low dark current in the near-infrared band. Even when no voltage is applied, the device still has stable near-infrared detection capability.

[0006] The technical solution of the present invention is:

[0007] A graphene nanoribbon-based infrared photodetector comprises, from bottom to top, an n-type gallium arsenide substrate, an n-type material contact electrode layer, a hafnium oxide layer, a p-type graphene nanoribbon layer, and a p-type material contact electrode layer.

[0008] Preferably according to the present invention, the thickness of the hafnium oxide layer is 5-20 nm.

[0009] Further preferably, the thickness of the hafnium oxide layer is 10 nm.

[0010] Preferably according to the present invention, the material of the p-type material contact electrode layer is Ti or Au, and the thicknesses are 5 nm and 40 nm respectively.

[0011] Preferably according to the present invention, the n-type material contact electrode layer is made of Ti, Pd, and Au, with thicknesses of 3 nm, 20 nm, and 40 nm, respectively.

[0012] The above-mentioned method for preparing the graphene nanoribbon-based infrared photoelectric detector comprises:

[0013] (1) Using n-type gallium arsenide as the n-type material layer and as the substrate, i.e., n-type gallium arsenide substrate;

[0014] (2) depositing a metal electrode on a partial area of ​​the n-type gallium arsenide substrate to obtain an n-type material contact electrode layer;

[0015] (3) depositing a hafnium oxide layer on the n-type material contact electrode layer using atomic layer deposition (ALD) technology;

[0016] (4) filtering the graphene nanoribbon suspension with an aqueous filter membrane, dissolving the aqueous filter membrane in an acetone solution, removing the graphene nanoribbon film, and covering the graphene nanoribbon film on the hafnium oxide layer, drying the sample at 40-60° C. for 1-2 h to fully dry the sample to obtain a p-type graphene nanoribbon layer, thereby obtaining a graphene nanoribbon / hafnium oxide / gallium arsenide sample;

[0017] (5) annealing the graphene nanoribbon / hafnium oxide / gallium arsenide sample in an inert gas atmosphere;

[0018] (6) Depositing a metal electrode on the graphene nanoribbon / hafnium oxide / gallium arsenide sample treated in step (5) to obtain a p-type material contact electrode layer.

[0019] Further preferably, in step (4), the p-type graphene nanoribbon layer is obtained after drying at 60° C. for 2 h.

[0020] Preferably according to the present invention, in step (3), the concentration of the graphene nanoribbon suspension is 0.01-10 mg / mL.

[0021] Preferably, according to the present invention, in step (4), the inert gas is pure argon or pure nitrogen, the annealing temperature is 300-600° C., and the annealing time is 2-4 hours.

[0022] Further preferably, in step (4), the annealing temperature is 300° C. and the annealing time is 2 h.

[0023] Preferably according to the present invention, in step (2) and step (6), the deposition method of the metal electrode includes but is not limited to electron beam evaporation, thermal evaporation, and magnetron sputtering.

[0024] The beneficial effects of the present invention are:

[0025] The photoelectric detector obtained by the preparation method provided by the present invention has a strong response to short-wave infrared light, and under the condition of no voltage being applied, the device still has a stable infrared light detection capability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the PL spectrum of graphene nanoribbon materials.

[0027] Figure 2 Schematic diagram of the structure of graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector.

[0028] Figure 3 Schematic diagram of the current-voltage curve of the graphene nanoribbon / hafnium oxide / gallium arsenide photodetector in the dark state and under 1064nm laser irradiation.

[0029] Figure 4 Schematic diagram of the dynamic photocurrent response curve of the graphene nanoribbon / hafnium oxide / gallium arsenide photodetector under different bias voltages at a light power of 1.6 μw.

[0030] 1. n-type gallium arsenide substrate, 2. n-type material contact electrode layer, 3. hafnium oxide layer, 4. p-type graphene nanoribbon layer, 5. p-type material contact electrode layer. DETAILED DESCRIPTION

[0031] The present invention will be further defined below in conjunction with the accompanying drawings and embodiments, but is not limited thereto.

[0032] Example 1

[0033] A graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector, such as Figure 2 As shown, from bottom to top, it includes an n-type gallium arsenide substrate 1, an n-type material contact electrode layer 2, a hafnium oxide layer 3, a p-type graphene nanoribbon layer 4, and a p-type material contact electrode layer 5.

[0034] Example 2

[0035] The graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector according to Example 1 is different in that:

[0036] The thickness of the hafnium oxide layer 3 is 5-20 nm. An oxide layer of suitable thickness can minimize dark current while having the least effect on photocurrent. However, when the oxide layer is too thick, it will delay the transmission of electrons and holes, resulting in a decrease in device performance.

[0037] Example 3

[0038] The graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector according to Example 1 is different in that:

[0039] The thickness of the hafnium oxide layer 3 is 10 nm.

[0040] The material of the n-type gallium arsenide substrate 1 is gallium arsenide, and the material of the p-type graphene nanoribbon layer 4 is graphene nanoribbon.

[0041] The material of the p-type material contact electrode layer 5 is Ti or Au. The size and position of the electrode are determined by electron beam coating or magnetron sputtering using a mask or laser direct writing. The thickness is 5 nm or 40 nm respectively.

[0042] The material of the n-type material contact electrode layer 2 is Ti, Pd, Au. The size and position of the electrode are determined by electron beam coating or magnetron sputtering using a mask or laser direct writing. The thicknesses are 3 nm, 20 nm, and 40 nm, respectively.

[0043] Example 4

[0044] The method for preparing the graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector described in any one of Examples 1-3 comprises:

[0045] (1) using n-type gallium arsenide as the n-type material layer and also as the substrate, i.e., n-type gallium arsenide substrate 1;

[0046] (2) depositing a metal electrode on a partial area of ​​the n-type gallium arsenide substrate 1 to obtain an n-type material contact electrode layer 2;

[0047] (3) depositing a hafnium oxide layer 3 on the n-type material contact electrode layer 2 using an atomic layer deposition (ALD) technique;

[0048] (4) filtering the graphene nanoribbon suspension with an aqueous filter membrane, dissolving the aqueous filter membrane in an acetone solution, removing the graphene nanoribbon film, and covering the graphene nanoribbon film on the hafnium oxide layer 3, drying the sample at 40-60° C. for 1-2 h to fully dry the sample, thereby obtaining a p-type graphene nanoribbon layer 4, and obtaining a graphene nanoribbon / hafnium oxide / gallium arsenide sample;

[0049] When filtering semiconductor graphene nanoribbons with aqueous filter membranes, be careful not to make them too thick and keep the thickness at tens of nanometers. Too thick a graphene nanoribbon film will affect the light absorption efficiency and cause the dark current of the device to be too large.

[0050] Figure 1 PL spectrum of graphene nanoribbon material; it can be seen that there is an obvious absorption peak at 686nm, which confirms the successful preparation of graphene nanoribbon. The preparation method of graphene nanoribbon suspension includes:

[0051] First, 50 mg of single-walled carbon nanotubes (SWCNTs, Sigma Aldrich) were annealed in air at 300°C for 30 minutes; then, immersed in 50 mL of concentrated sulfuric acid for 2 hours; then, 25 mg of KMnO4 (Sigma Aldrich) was added to the mixture and stirred for 2 hours; then stirred at 45°C for 30 minutes until the KMnO4 was completely consumed; the solution mixture was poured into 200 mL of ice deionized water, and then filtered with a mixed fiber membrane with a pore size of 0.45 μm, and the separated SWCNTs were washed with a large amount of water and dried in the air. 20 mg of dried SWCNTs were dispersed in 200 mL of 1% sodium dodecylbenzene sulfonate (Sigma Aldrich) solution, and then ultrasonicated for 180 minutes to obtain a graphene nanoribbon suspension.

[0052] (5) annealing the graphene nanoribbon / hafnium oxide / gallium arsenide sample in an inert gas atmosphere;

[0053] (6) Depositing a metal electrode on the graphene nanoribbon / hafnium oxide / gallium arsenide sample treated in step (5) to obtain a p-type material contact electrode layer 5.

[0054] In step (3), the concentration of the graphene nanoribbon suspension is 0.01-10 mg / mL. Too high a concentration of the graphene nanoribbon suspension will result in excessive carbon nanotube content in the solution, affecting the quality of the subsequent graphene nanoribbon film.

[0055] In step (4), the inert gas is pure argon or pure nitrogen, the annealing temperature is 300-600° C., and the annealing time is 2-4 hours. Impurities (such as oxygen-containing groups) on the graphene nanoribbon film are removed to facilitate subsequent testing.

[0056] Example 5

[0057] The method for preparing the graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector according to Example 4 is different in that:

[0058] In step (4), after drying at 60° C. for 2 h, a p-type graphene nanoribbon layer 4 is obtained.

[0059] In step (4), the annealing temperature is 300° C. and the annealing time is 2 h.

[0060] In step (2) and step (6), the deposition method of the metal electrode includes but is not limited to electron beam evaporation, thermal evaporation, and magnetron sputtering.

[0061] Figure 3 The current-voltage curves of the graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector in the dark state and under 1064nm laser irradiation are shown in Figure 2. It can be seen that the current of the photodetector under laser irradiation is significantly greater than the current in the dark state, indicating that the photodetector has a significant light response to the 1064nm laser.

[0062] Figure 4 The following is a graph of the dynamic photocurrent response curve of the graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector at -1, -3, and -5 V under a light power of 1.8 μW. It can be seen that as the bias voltage changes, the photocurrent of the photodetector gradually increases, with a fast response and high sensitivity, successfully realizing the detection of short-wave infrared light.

[0063] The graphene nanoribbon / hafnium oxide / gallium arsenide infrared photodetector of the present invention overcomes the relatively small response of the photodetection in the prior art, so that the photodetector of the present invention has an extremely low dark current, and achieves high response and high sensitivity in the short-wave infrared through the interaction between the graphene nanoribbon and the gallium arsenide heterojunction, so that the graphene nanoribbon vertical heterojunction photodetector of the present invention has excellent detection effect in the near-infrared band.

Claims

1. A graphene nanoribbon infrared photodetector, characterized in that: From bottom to top, it includes an n-type gallium arsenide substrate, an n-type material contact electrode layer, a hafnium oxide layer, a p-type graphene nanoribbon layer, and a p-type material contact electrode layer.

2. The graphene nanoribbon infrared photodetector according to claim 1, characterized in that: The thickness of the hafnium oxide layer is 5-20 nm.

3. The graphene nanoribbon infrared photoelectric detector according to claim 2, characterized in that: The thickness of the hafnium oxide layer is 10 nm.

4. The graphene nanoribbon infrared photodetector according to claim 1, characterized in that: The p-type material contact electrode layer is made of Ti and Au, with thicknesses of 5 nm and 40 nm respectively.

5. The graphene nanoribbon infrared photoelectric detector according to claim 1, characterized in that: The n-type material contact electrode layer is made of Ti, Pd, and Au, and has thicknesses of 3 nm, 20 nm, and 40 nm, respectively.

6. The method for preparing a graphene nanoribbon infrared photodetector according to any one of claims 1 to 5, characterized in that: include: (1) Using n-type gallium arsenide as the n-type material layer and as the substrate, i.e., n-type gallium arsenide substrate; (2) depositing a metal electrode on a partial area of ​​the n-type gallium arsenide substrate to obtain an n-type material contact electrode layer; (3) depositing a hafnium oxide layer on the n-type material contact electrode layer using an atomic layer deposition technique; (4) filtering the graphene nanoribbon suspension with an aqueous filter membrane, dissolving the aqueous filter membrane in an acetone solution, removing the graphene nanoribbon film, and covering the graphene nanoribbon film on the hafnium oxide layer, drying the sample at 40-60° C. for 1-2 h to fully dry the sample to obtain a p-type graphene nanoribbon layer, thereby obtaining a graphene nanoribbon / hafnium oxide / gallium arsenide sample; (5) annealing the graphene nanoribbon / hafnium oxide / gallium arsenide sample in an inert gas atmosphere; (6) Depositing a metal electrode on the graphene nanoribbon / hafnium oxide / gallium arsenide sample treated in step (5) to obtain a p-type material contact electrode layer.

7. The method for preparing a graphene nanoribbon infrared photodetector according to claim 6, characterized in that: In step (4), after drying at 60° C. for 2 h, a p-type graphene nanoribbon layer is obtained.

8. The method for preparing a graphene nanoribbon infrared photodetector according to claim 6, characterized in that: In step (3), the concentration of the graphene nanoribbon suspension is 0.01-10 mg / mL.

9. The method for preparing a graphene nanoribbon infrared photodetector according to claim 6, characterized in that: In step (4), the inert gas is pure argon or pure nitrogen, the annealing temperature is 300-600° C., and the annealing time is 2-4 h; Further preferably, in step (4), the annealing temperature is 300° C. and the annealing time is 2 h.

10. The method for preparing a graphene nanoribbon infrared photodetector according to claim 6, characterized in that: In step (2) and step (6), the deposition method of the metal electrode includes electron beam evaporation, thermal evaporation, and magnetron sputtering.