Expanded bulk silicon anode material

By immersing the silicon blank in the molten salt and applying a potential, alkali metal ions are driven into the silicon lattice to form a high-performance silicon anode, which solves the problems of limited capacity and reduced performance of silicon anode in lithium-ion batteries, and achieves high energy storage and long-term Cycle life.

CN118943294APending Publication Date: 2024-11-12FORD GLOBAL TECH LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410476123.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-04
Filing Date
2024-04-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The capacity of graphite anode in traditional lithium-ion batteries is limited. The volume expansion of the silicon anode during the charging/discharge cycle leads to loss of electrical contact, resulting in degradation of performance. The existing methods to improve the performance of silicon anode are complex and time-consuming.

Method used

The bulk silicon blank is immersed in the molten salt, and the negative potential is applied to the silicon blank and the positive potential is applied to the container of the sacrificial electrode or molten salt, which initiates an electrolytic reaction, driving alkali metal ions such as sodium or lithium into the silicon lattice to form Anode with ductility and high energy storage capacity.

Benefits of technology

By controlling the temperature and potential difference of molten salt, a high-performance silicon anode is formed, which improves the energy storage capacity and cycle life, simplifies the production process, and avoids the rupture of the silicon anode and the poor cycle life problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943294A_ABST
    Figure CN118943294A_ABST
Patent Text Reader

Abstract

The present disclosure provides an expanded bulk silicon anode material. A method for making an electrode involves: forming a molten salt; a negative terminal of a direct current power source is attached to the silicon blank and a positive terminal of the direct current power source is attached to a sacrificial electrode or a container of the molten salt. The method also involves immersing the silicon blank in the molten salt such that an electrolytic reaction drives alkali metal ions into the lattice of the silicon blank.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to electrode materials for lithium-ion batteries. Background Art

[0002] As demand for portable electronic devices, electric vehicles, and renewable energy continues to grow, energy storage is a consideration. Batteries are common energy storage devices that sometimes rely on electrodes. Electrodes can efficiently store and release electrical charge. Summary of the invention

[0003] A method for forming a silicon anode used in batteries and other energy storage devices involves placing a bulk silicon blank into a container containing a molten salt, while applying a negative charge to the silicon blank and a positive charge to a sacrificial electrode or container of the molten salt. This causes an electrolytic reaction, thereby driving alkali metal ions from the molten salt into the silicon blank lattice. After a set time, the anode is removed from the molten salt and cooled. A current collector may be placed on the anode, and some of the alkali metal ions remain in the anode after discharge. The temperature of the molten salt is at least 500 degrees Celsius, and the alkali metal ions used may be sodium or lithium. The silicon blank may be a silicon wafer.

[0004] Alternatively, a method for forming an electrode for use in a battery or other energy storage device involves heating sodium hydroxide or lithium hydroxide until it becomes a molten salt, then attaching a DC power supply to a silicon wafer and a sacrificial electrode or container of the molten salt. The silicon wafer is lowered into the molten salt, causing the sodium or lithium ions to be driven into the silicon and form an ion-laden anode. After the anode reaches its maximum capacity, it is lifted out of the molten salt and allowed to cool. BRIEF DESCRIPTION OF THE DRAWINGS

[0005] Figure 1A is a graph showing the relationship between Young's modulus and the presence of lithium in silicon.

[0006] Figure 1B is a graph showing the ultimate strength of intrinsic silicon over the entire temperature range.

[0007] Figure 1C is a graph showing the temperature dependence of the thermal conductivity and electrical conductivity of silicon.

[0008] Figure 2 is a flow chart of a method for forming a silicon anode material.

[0009] Figure 3 is a schematic diagram of a lithium-ion battery. DETAILED DESCRIPTION

[0010] Embodiments are described herein. However, it should be understood that the disclosed embodiments are merely examples and that other embodiments may take various and alternative forms. The drawings are not necessarily drawn to scale. Some features may be enlarged or minimized to show details of particular components. Therefore, the specific structural details and functional details disclosed herein should not be interpreted as limiting, but merely as a representative basis for teaching those skilled in the art.

[0011] The various features shown and described with reference to any one of the accompanying drawings may be combined with features shown in one or more other drawings to produce embodiments not explicitly shown or described. The combinations of features shown provide representative embodiments for typical applications. However, for specific applications or implementations, various combinations and modifications of features consistent with the teachings of the present disclosure may be desired.

[0012] Traditionally, graphite has been used as an anode material for lithium-ion batteries. However, the capacity of graphite anodes can be limited, and higher capacity anode materials are needed to improve battery performance. Silicon is a promising candidate material for anodes due to its high theoretical capacity for lithium-ion storage (approximately ten times that of graphite).

[0013] Charge / discharge cycling of silicon anodes can cause capacity to decrease over time. This degradation is due to volume expansion of silicon during lithiation, which causes the material to lose electrical contact. To overcome this limitation, various methods have been proposed to improve the performance of silicon anodes, including nanostructuring, alloying with other elements, and using carbon coatings. However, these methods are generally complex and time consuming, and a simple and effective method for producing high-performance silicon anodes is needed.

[0014] Silicon-based anodes for batteries show great promise in terms of energy storage capacity and performance. However, conventional methods of producing silicon anodes can be complex, leading to potential problems such as cracking and poor cycle life. Novel methods of forming electrodes have been developed to address these challenges and enhance overall battery performance. In one example, a bulk silicon billet is immersed in a molten salt next to a sacrificial electrode. A negative potential is applied to the silicon billet, a positive potential is applied to the silicon billet, and a positive potential is simultaneously applied to the sacrificial electrode or container holding the molten salt. The simultaneous application of the potential and immersion in the molten salt initiates an electrolytic reaction, driving alkali metal ions such as sodium or lithium ions from the molten salt into the lattice of the silicon billet.

[0015] The method facilitates the formation of anodes with ductile deformation that can accommodate the stresses and strains induced by the insertion of alkali metal ions. By carefully controlling the process parameters, including the temperature of the molten salt, the predetermined immersion time, the applied DC voltage level, and the choice of alkali metal ions, this method allows the formation of high-performance silicon anodes with improved energy storage capacity and cycle life. Such advances in electrode manufacturing have the potential to further advance the field of energy storage and pave the way for the development of more efficient, longer-lasting batteries for a wide range of applications.

[0016] Figure 1A A graphical representation of the relationship between Young's modulus and the presence of lithium in silicon is shown, highlighting the changes in mechanical properties that occur during the process of lithium insertion into a silicon material. This relationship may help understand the mechanical stability and performance of silicon when used as an anode material. The x-axis represents the presence of lithium in the silicon lattice. The y-axis represents Young's modulus, a measure of the stiffness of a material, expressed in units of pressure, gigapascals (GPa). The graph shows that when lithium ions are inserted into the silicon lattice, the Young's modulus of the silicon material decreases, indicating an increase in ductility and a decrease in stiffness.

[0017] Figure 1B A graphical representation of the ultimate strength of silicon as a function of temperature is shown, highlighting the temperature-dependent mechanical properties of silicon. Knowing the ultimate strength of silicon over the entire temperature range is helpful when ensuring mechanical stability and performance under a variety of operating conditions. Figure 1B In the diagram, the x-axis represents the temperature in degrees Celsius (°C). The y-axis represents the pressure of silicon in Nm 2 ) is shown in Figure 1. The graph shows that at around 550 degrees Celsius, the ultimate strength of silicon increases greatly. The ultimate strength of silicon at and above this temperature ranges from brittle cleavage to one of ductile ultimate strength.

[0018] Figure 1C A graphical representation of the temperature dependence of both the thermal and electrical conductivity of silicon is shown. Figure 1C In Figure 1, the x-axis represents temperature in Kelvin (K), and the y-axis represents both the thermal conductivity and electrical conductivity of silicon. Thermal conductivity is expressed in Watts per meter-Kelvin (W / mK), which is a measure of a material's ability to transfer heat. Electrical conductivity is a measure of a material's ability to conduct an electric current, represented by the symbol σ, and is expressed in Ohm-meters (OM -1 M -1 ) is expressed in units of . The two curves show how the thermal conductivity and electrical conductivity in silicon vary with temperature. While the thermal conductivity of silicon is temperature dependent, decreasing with increasing temperature, the electrical conductivity of silicon is largely independent of temperature.

[0019] View now Figure 2, at box 10, a molten salt solution is prepared and the silicon blank is attached to a power source. In the first step of the process, sodium hydroxide or lithium hydroxide is heated to a temperature of at least 500 degrees Celsius, resulting in the formation of a molten salt. By attaching the negative terminal of a direct current (DC) power source to the silicon wafer, a silicon wafer that can be used as a bulk silicon blank is prepared for the process. At the same time, the positive terminal of the DC power source is attached to a sacrificial electrode or a container containing the molten salt. This setup establishes an electrochemical cell in which the silicon wafer acts as a working electrode and the sacrificial electrode or container acts as a counter electrode. During the electrode formation process, the temperature of the molten salt is maintained at at least 500 degrees Celsius to ensure that the silicon is in its ductile phase, such as Figure 1B When silicon is in its ductile phase, it exhibits increased flexibility and deformability, which facilitates the incorporation of alkali metal ions (such as sodium or lithium ions) into its lattice structure.

[0020] In block two 12, the silicon wafer is carefully lowered into the molten salt while a DC power supply applies a negative potential to the silicon wafer and a positive potential to the sacrificial electrode or container. This potential difference causes an electrolytic reaction between the molten salt and the silicon wafer, thereby driving alkali metal ions (possibly sodium ions or lithium ions) from the molten salt into the lattice of the silicon wafer. This process continues for a predetermined period of time, during which the silicon wafer undergoes ductile deformation, resulting in the formation of an anode with maximum capacity for alkali metal ions.

[0021] The predetermined time period may correspond to an immersion duration that allows the silicon wafer to reach its maximum holding capacity, thereby ensuring that the electrolytic reaction between the molten salt and the silicon wafer effectively drives the alkali metal ions into the lattice of the silicon wafer. The predetermined time period may be determined experimentally based on the composition and weight percentage of the molten salt, the type of alkali metal ions, the size of the silicon blank, and specific operating conditions including temperature and current density. By varying these factors during experimental trials and monitoring the performance of the ion-loaded silicon anode material, an optimal predetermined time period may be established. Such trials may involve measuring the amount of alkali metal ions incorporated into the silicon lattice, the total capacity of the anode, or other relevant performance indicators.

[0022] Alternatively, the silicon wafer can be immersed until it reaches its maximum holding capacity, which means that the lattice of the silicon wafer is loaded with ions. The maximum holding capacity can be similarly determined experimentally by known methods. Once a predetermined period of time has passed and the anode has reached its maximum holding capacity, in frame three 14, the anode is removed from the molten salt and allowed to cool to room temperature. After cooling, the anode is assembled into an electrochemical cell by arranging a current collector in contact with the anode. The assembly may also include other components, such as separators, cathodes, and electrolytes, depending on the specific design of the cell. The resulting electrochemical cell characterized by the silicon anode material can be used for various energy storage applications, such as batteries for electric vehicles or portable electronic devices.

[0023] View now Figure 3 , an assembled battery cell 16 is shown. The battery cell 16 is designed for efficient energy storage and utilizes the novel silicon anode material 18 as described above. The battery cell 16 is composed of several components, including a positive current collector 20, a negative current collector 22, a ceramic insulator 24, a cathode 26, an anode 28, an insulating sheath 30, and a molten salt electrolyte 32.

[0024] In the assembled battery cell 16, the ion-loaded silicon anode 28 may be in contact with a separator (not shown), which is a thin layer that separates the cathode 26 and the anode 28 and prevents direct contact between them. The silicon anode 22 may also be in contact with a molten salt electrolyte 32 and a negative current collector 22. Because the anode 28 is the result of the novel process described herein, it is particularly ion-loaded. The negative current collector 22 is responsible for facilitating the transfer of electrons between the anode 28 and the external circuit 34 during the discharge process and the charging process.

[0025] The cathode 26 may be in contact with a separator (not shown), a molten salt electrolyte 32, and a positive current collector 20. Like the negative current collector 22, the positive current collector 20 ensures efficient electron transfer between the cathode 26 and the external circuit 34. The cathode 26 may be any metal oxide, such as lithium cobalt oxide (LCO), lithium iron phosphate (LFP), or lithium manganese oxide (LMO). The ceramic insulator 24 is positioned between the positive electrode 26 and the negative electrode 28 to prevent electrical short circuits and maintain physical separation therebetween. The ceramic insulator 24 may be composed of materials such as zirconium oxide, aluminum oxide, or other suitable ceramic materials known for their excellent insulating properties and stability at high temperatures.

[0026] Molten salt electrolyte 32 is contained in the battery cell 16, thereby filling the space between anode 28 and cathode 26. Electrolyte 32 is responsible for promoting ion transport of alkali metal ions between anode 28 and cathode 26 during charging and discharging processes. Molten salt electrolyte 32 can be derived from sodium hydroxide or lithium hydroxide, or from other suitable salts that ensure effective ionic conductivity. Insulating sheath 30 is used to encase the assembled battery cell 16, thereby providing both mechanical protection and electrical insulation. Insulating sheath 30 can be made of a non-conductive and thermally stable material (such as a polymer or ceramic) that can withstand the operating temperature and working conditions of electrochemical battery cell 16.

[0027] The battery cells 16 can be assembled to form a battery pack. During operation of the assembled battery cells 16, the load is connected to the external circuit 34, thereby drawing energy from the battery cells 16. When the battery cells 16 are discharged, alkali metal ions (such as sodium ions or lithium ions) migrate from the anode 28 through the molten salt electrolyte 32 toward the cathode 26. At the same time, electrons flow from the negative current collector 22 through the external circuit 34 to the positive current collector 20, thereby supplying power to the load. The efficient movement of ions within the battery cell 16 and its transfer to the load helps maintain optimal performance and energy storage capacity.

[0028] During the charging process, an external circuit 34 supplies energy to the battery cell 16, driving the alkali metal ions from the cathode 26 back into the anode 28 through the molten salt electrolyte 32. The ceramic insulator 24 maintains the separation of the electrodes 26, 28 while enabling ion flow between the electrodes 26, 28. By optimizing the design and operation of the assembled battery cell 16, efficient ion migration and energy transfer can be achieved, resulting in a high-performance energy storage device capable of delivering power to a variety of loads under different operating conditions.

[0029] The algorithm, method or process disclosed herein may be delivered to or implemented by a computer, controller or processing device, which may include any dedicated electronic control unit or programmable electronic control unit. Similarly, the algorithm, method or process can be stored in many forms as data and instructions that can be executed by a computer or controller, including but not limited to information permanently stored on non-writable storage media such as read-only memory devices and information that can be changed and stored on writable storage media such as optical disks, random access memory devices or other magnetic and optical media. The algorithm, method or process can also be implemented by a software executable object. Alternatively, the algorithm, method or process can be implemented in whole or in part using a combination of suitable hardware components or hardware, software and firmware components, such as a combination of application-specific integrated circuits, field programmable gate arrays, state machines or other hardware components or devices, or firmware, hardware and software components.

[0030] Although exemplary embodiments are described above, these embodiments are not intended to describe all possible forms covered by the claims. The words used in the specification are words of description rather than limitation, and it should be understood that various changes can be made without departing from the spirit and scope of these disclosed materials.

[0031] As previously mentioned, the features of the various embodiments may be combined to form additional embodiments of the invention that may not be explicitly described or shown. Although various embodiments may have been described as providing advantages or being preferred over other embodiments or prior art implementations with respect to one or more desired characteristics, it will be appreciated by those of ordinary skill in the art that one or more features or characteristics may be compromised to achieve desired overall system properties, depending on the specific application and implementation. These properties may include, but are not limited to, strength, durability, marketability, appearance, packaging, size, serviceability, weight, manufacturability, ease of assembly, and the like. For this reason, embodiments that are described as being less desirable than other embodiments or prior art implementations with respect to one or more characteristics are within the scope of the present disclosure and may be desirable for a particular application.

[0032] According to the present invention, a method for forming an electrode comprises: while applying a negative potential to a bulk silicon blank and applying a positive potential to a sacrificial electrode or a container containing a molten salt, immersing the silicon blank and the sacrificial electrode in the molten salt for a predetermined period of time, so that the electrolysis reaction of the molten salt with the silicon blank drives the alkali metal ions from the molten salt into the crystal lattice of the silicon blank, thereby resulting in the formation of an anode and its ductile deformation; and after the predetermined period of time, removing the anode from the molten salt to cool the anode.

[0033] In one aspect of the invention, the method comprises arranging a current collector in contact with the anode.

[0034] In one aspect of the invention, the alkali metal ions are driven into the crystal lattice such that after discharge, at least some of the alkali metal ions remain in the crystal lattice.

[0035] In one aspect of the invention, the temperature of the molten salt is at least 500 degrees Celsius.

[0036] In one aspect of the present invention, the alkali metal ion is a sodium ion or a lithium ion.

[0037] In one aspect of the invention, the predetermined period of time is sufficient to allow the anode to reach maximum holding capacity.

[0038] In one aspect of the invention, the method comprises heating sodium hydroxide or lithium hydroxide to form the molten salt.

[0039] In one aspect of the present invention, the bulk silicon ingot is a silicon wafer.

[0040] According to the present invention, a method for forming an electrode includes: heating sodium hydroxide or lithium hydroxide to at least 500 degrees Celsius to form a molten salt; attaching the negative terminal of a direct current power supply to a silicon wafer and attaching the positive terminal of the direct current power supply to a sacrificial electrode or the molten salt; lowering the silicon wafer with the negative terminal and the positive terminal attached into the molten salt to drive sodium ions or lithium ions into the lattice of the silicon wafer, thereby forming an ion-carrying anode; and after the ion-carrying anode reaches a maximum holding capacity, lifting the ion-carrying anode out of the molten salt to cool the ion-carrying anode.

[0041] In one aspect of the invention, the method comprises arranging a current collector in contact with the ion-carrying anode.

[0042] In one aspect of the invention, the alkali metal ions are driven into the crystal lattice such that after discharge, at least some of the alkali metal ions remain in the crystal lattice.

[0043] According to the present invention, a method for forming an electrode includes: preparing a molten salt by heating an alkali metal hydroxide to a temperature of at least 500 degrees Celsius; simultaneously applying a negative potential to a bulk silicon blank and applying a positive potential to a sacrificial electrode or a container containing the molten salt; and immersing the silicon blank and the sacrificial electrode in the molten salt to induce an electrolysis reaction, thereby driving alkali metal ions from the molten salt into the crystal lattice of the silicon blank, thereby resulting in the formation of an ion-loaded anode.

[0044] In one aspect of the invention, the method comprises, after a predetermined period of time, subsequently removing the ion-loaded anode from the molten salt to allow it to cool.

[0045] In one aspect of the invention, the method comprises arranging a current collector in contact with the ion-carrying anode.

[0046] In one aspect of the invention, the alkali metal ions are driven into the crystal lattice such that after discharge, at least some of the alkali metal ions remain in the crystal lattice.

[0047] In one aspect of the present invention, the alkali metal ion is a sodium ion or a lithium ion.

Claims

1. A method for forming an electrode, the method comprising: While applying a negative potential to a bulk silicon ingot and a positive potential to a sacrificial electrode or a container containing a molten salt, immersing the silicon ingot and the sacrificial electrode in the molten salt for a predetermined period of time, such that an electrolytic reaction of the molten salt with the silicon ingot drives alkali metal ions from the molten salt into the crystal lattice of the silicon ingot, thereby causing the formation of an anode and ductile deformation thereof; as well as After the predetermined period of time, the anode is removed from the molten salt to cool the anode.

2. The method of claim 1, further comprising placing a current collector in contact with the anode.

3. The method of claim 1, wherein the alkali metal ions are driven into the crystal lattice such that after discharge, at least some of the alkali metal ions remain in the crystal lattice.

4. The method of claim 1, wherein the temperature of the molten salt is between 500 degrees Celsius and 550 degrees Celsius. The method of claim 1 , wherein the alkali metal ion is a sodium ion or a lithium ion.

6. The method of claim 1, wherein the predetermined period of time is sufficient to allow the anode to reach maximum holding capacity.

7. The method of claim 1, further comprising heating sodium hydroxide or lithium hydroxide to form the molten salt. The method of claim 1 , wherein the bulk silicon ingot is a silicon wafer.

9. A method for forming an electrode, the method comprising: heating sodium hydroxide or lithium hydroxide to between 500 degrees Celsius and 550 degrees Celsius to form a molten salt; attaching a negative terminal of a DC power source to the silicon wafer and attaching a positive terminal of the DC power source to a sacrificial electrode or the molten salt; lowering the silicon wafer with the negative terminal and the positive terminal attached into the molten salt to drive sodium or lithium ions into the crystal lattice of the silicon wafer, thereby resulting in the formation of an ion-loaded anode; as well as After the ion-carrying anode reaches a maximum holding capacity, the ion-carrying anode is lifted out of the molten salt to cool the ion-carrying anode.

10. The method of claim 9, further comprising placing a current collector in contact with the ion-carrying anode.

11. The method of claim 9, wherein the alkali metal ions are driven into the crystal lattice such that after discharge, at least some of the alkali metal ions remain in the crystal lattice.

12. A method for forming an electrode, the method comprising: preparing a molten salt by heating an alkali metal hydroxide to a temperature in the range of 500 degrees Celsius to 550 degrees Celsius; Simultaneously, a negative potential is applied to the bulk silicon blank, and a positive potential is applied to the sacrificial electrode or the container containing the molten salt; as well as The silicon ingot and the sacrificial electrode are immersed in the molten salt to initiate an electrolytic reaction, thereby driving alkali metal ions from the molten salt into the crystal lattice of the silicon ingot, resulting in the formation of an ion-loaded anode.

13. The method of claim 12, further comprising, after a predetermined period of time, subsequently removing the ion-loaded anode from the molten salt to allow it to cool.

14. The method of claim 12, further comprising placing a current collector in contact with the ion-carrying anode.

15. The method of claim 12, wherein the alkali metal ions are driven into the crystal lattice such that after discharge, at least some of the alkali metal ions remain in the crystal lattice.