Flexible supporting nickel phthalocyanine composite carbon electrode and preparation method and application thereof

Through the preparation of flexible support nickel phthalocyanine composite carbon electrode, the problems of poor reversibility and complex preparation of existing Li-SOCl2 batteries are solved, and the cycle life and reversible capacity of the battery are improved. It is suitable for smart devices and is more stable and Highly efficient battery performance.

CN118943298APending Publication Date: 2024-11-12ZHENGZHOU YILONG INTELLIGENT INNOVATION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410987778.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The cathode reaction of existing rechargeable Li-SOCl2 batteries is poor, and the complex oxidation-reduction interface hinders the transmission of electrons and Li+ ions, resulting in a short battery cycle life, and a complex preparation process and is unable to provide large-area discharge capacity, resulting in the battery. Poor resilience and potentially dangerous.

Method used

Using flexible supported nickel phthalocyanine composite carbon electrode, a flexible electrode with excellent oxidation-reduction interface was prepared by mixing activated carbon-loaded nickel phthalocyanine composite material with acetylene black by rolling pressure method, which improved the adsorption capacity and cycle life of Cl2. Reduces the internal resistance of the battery.

Benefits of technology

It improves the cycle life and reversible capacity of the battery, reduces the attenuation rate of the battery, enhances the stability and volume effect of the flexible electrodes, is suitable for smart devices, and has a simple process, good stability and high yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943298A_ABST
    Figure CN118943298A_ABST
Patent Text Reader

Abstract

The invention discloses a flexible support nickel phthalocyanine composite carbon electrode and a preparation method and application thereof, and the method comprises the steps: 1, mixing pyropitch activated carbon, phthalic anhydride, urea, nickel chloride hexahydrate and ammonium molybdate tetrahydrate, and grinding to obtain a mixture A; 2, sintering the mixture A in an air atmosphere, cooling, grinding, soaking, cleaning and drying to obtain an activated carbon loaded nickel phthalocyanine composite material; 3, uniformly mixing the polytetrafluoroethylene emulsion with deionized water to obtain a polytetrafluoroethylene emulsion diluent; 4, acetylene black and the activated carbon loaded nickel phthalocyanine composite material are uniformly mixed to obtain a mixture B, the mixture B is added into a polytetrafluoroethylene emulsion diluent, a trace amount of absolute ethyl alcohol is added, uniform grinding and drying are performed, and a polytetrafluoroethylene cross-linked composite carbon cathode mixture is obtained; and 5, soaking the polytetrafluoroethylene cross-linked composite carbon cathode mixture in absolute ethyl alcohol, rolling and drying to obtain the flexible supporting nickel phthalocyanine composite carbon electrode, thereby prolonging the cycle life of the battery and improving the reversible capacity of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rechargeable lithium / thionyl chloride batteries, and in particular is a flexible supported nickel phthalocyanine composite carbon electrode and a preparation method and application thereof. Background Art

[0002] In recent years, with the popularity of various electronic products, the requirements for battery performance have become increasingly higher. As a battery with the highest specific energy, lithium / thionyl chloride batteries have attracted widespread attention. 2 Batteries are already relatively mature, but how to convert them into rechargeable Li-SOCl 2 Batteries remain a huge challenge.

[0003] Existing rechargeable Li-SOCl 2 The cathode of the battery usually adopts a porous carbon electrode. Its excellent conductivity is conducive to the infiltration of electrolyte and the loading of more discharge products, such as lithium chloride and sulfur. However, lithium chloride is insoluble in electrolyte. During the discharge process, the surface of the carbon cathode is gradually covered by blocky lithium chloride particles, which makes it impossible for metallic lithium to react with the reactant SOCl. 2 contact, resulting in premature termination of battery discharge; at the same time, the existing Li / SOCl 2 The battery not only has poor cathode reaction reversibility, but also complex redox interface hinders the electron and Li + During the charging process, LiCl is electrochemically oxidized to form Cl 2 , and then partially regenerated into SOCl through a series of chemical reactions 2 During the oxidation process, the oxidation rate is low, which shortens the cycle life of the battery.

[0004] In addition, in the preparation of Li / SOCl 2 In the process of preparing the battery cathode, the cathode mixture is usually dissolved in the solvent ethanol to prepare a slurry, and then dripped on the nickel foam collector. After drying and rolling, a rigid positive electrode of the lithium / thionyl chloride battery is obtained. However, this method has the problems of complex process, poor electrode uniformity and inability to provide a large area discharge capacity. The prepared rigid positive electrode has poor toughness and no volume effect. The Cl generated during the charging process 2 The expansion of the battery volume not only increases the resistance and deteriorates the battery cycle performance, but also poses a potential hazard, thus limiting the rechargeable Li / SOCl 2 Battery applications. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a flexible supported nickel phthalocyanine composite carbon electrode and a preparation method and application thereof, which not only has good uniformity and high yield, but also accelerates the decomposition of LiCl in the carbon coating and the pores, and improves the Cl 2 The adsorption capacity of the battery is improved, thereby improving the cycle life and reversible capacity of the battery.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a flexible supported nickel phthalocyanine composite carbon electrode comprises the following steps:

[0008] Step 1, mixing and grinding pyroasphalt activated carbon, phthalic anhydride, urea, nickel chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of (0.1-0.3):(0.68-0.85):(1.08-1.68):(0.45-0.88):(0.12-0.21) to obtain a mixture A;

[0009] Step 2, placing the mixture A into a muffle furnace, heating the mixture from room temperature to 130-160° C. at a heating rate of 5-10° C. / min in an air atmosphere and keeping the temperature for 0.5-2 h, then heating the mixture to 260-290° C. at a heating rate of 5-10° C. / min, keeping the temperature for 1-3 h, cooling the mixture naturally to room temperature, grinding, soaking, washing and drying the mixture in turn to obtain an activated carbon-supported nickel phthalocyanine composite material;

[0010] Step 3, mixing a polytetrafluoroethylene emulsion having a solid content of 60% with deionized water in a mass ratio of (0.02-0.03):(1.167-1.5), stirring evenly, and obtaining a polytetrafluoroethylene emulsion dilution;

[0011] Step 4, acetylene black and activated carbon-supported nickel phthalocyanine composite material are mixed in a mass ratio of 100:(4-8), stirred evenly to obtain a mixture B, and the mixture B is added to a polytetrafluoroethylene emulsion diluent in a mass ratio of 1:4.7, and then a trace amount of anhydrous ethanol is added, ground evenly, and then dried to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;

[0012] Step 5: After soaking the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol, the mixture is gradually rolled and dried using a roller press to obtain a flexible supported nickel phthalocyanine composite carbon electrode.

[0013] Furthermore, the soaking in step 2 is performed by soaking in deionized water for at least 12 hours, removing the upper suspended matter first, then changing the water for soaking, and repeating for 3 times.

[0014] Furthermore, the cleaning in step 2 is firstly performed with anhydrous ethanol for 2 to 4 times, and then with deionized water for 1 to 5 times.

[0015] Furthermore, the drying in step 2 is carried out at 60 to 150° C. for 12 to 24 hours.

[0016] Furthermore, the drying in step 4 is performed by using a muffle furnace or an oven, heating the temperature from room temperature to 160-200° C. at a heating rate of 5-10° C. / min, and drying for 4-24 hours.

[0017] Furthermore, in step 5, the polytetrafluoroethylene cross-linked composite carbon cathode mixture is immersed in anhydrous ethanol for 20 minutes to 24 hours.

[0018] Furthermore, the process of step 5 of gradually rolling the nickel phthalocyanine composite carbon electrode using a roller press is as follows: first, anhydrous ethanol is extruded with a small pressure using a roller press, and then cut into pieces, and then pressed in sequence with working thicknesses of 1.75-2 mm, 1.25-1.5 mm, 0.75-1.0 mm, and 0.25-0.75 mm to obtain a flexible supported nickel phthalocyanine composite carbon electrode with a thickness of 0.25-0.75 mm.

[0019] Furthermore, the drying in step 5 is carried out at 50-130° C. for 2-24 hours.

[0020] A flexible supported nickel phthalocyanine composite carbon electrode.

[0021] Application of flexible supported nickel phthalocyanine composite carbon electrode as positive electrode for rechargeable lithium / thionyl chloride batteries.

[0022] Compared with the prior art, the present invention has the following technical effects:

[0023] The present invention prepares phthalocyanine by a metal template method. As a macrocyclic compound with a large π structure conjugated system, aromatic π electrons are conjugated on the entire phthalocyanine ring, have both electron-donating and electron-accepting properties, and can be used as a good electron donor and acceptor. The conjugated macromolecule has a highly planar property, and the catalytic reaction can occur at the axial position of the plane, and has excellent catalytic performance. Moreover, the holes in the ring can accommodate metal elements to form a complex, and have good thermal stability and chemical stability. The phthalocyanine is loaded on pyro-asphalt activated carbon with rich pore structure, high specific surface area and rich oxygen-containing functional groups to synthesize an activated carbon-loaded nickel phthalocyanine composite material, which has a loose and porous morphology and an excellent oxidation-reduction interface. The phthalocyanine is used as a catalyst to reduce the close stacking of LiCl and improve the Cl 2The adsorption capacity of acetylene black was improved by mixing it with acetylene black with good conductivity to make a slurry, and a flexible supported nickel phthalocyanine composite carbon electrode was prepared by a roller pressing method. This not only solved the problem of uneven catalyst mixing in the process of preparing the positive electrode of rechargeable lithium / thionyl chloride battery by the existing slurry titration method, but also, because acetylene black and activated carbon-supported nickel phthalocyanine composite materials have similar morphologies, they are compatible as the main components of the carbon cathode, can form a stable structure, and reduce the rechargeable Li / SOCl 2 The volume of the battery expands and contracts during the charge and discharge process, thereby reducing the battery's attenuation rate and improving the battery's cycle stability. Furthermore, the conductive network formed by the combination of acetylene black and activated carbon-loaded nickel phthalocyanine composite material not only helps the rapid transmission of electrons in the battery and reduces the battery's internal resistance, but also helps the decomposition of the carbon coating and LiCl in the pores during the charging process, thereby improving the battery's cycle life and reversible capacity.

[0024] The present invention soaks the polytetrafluoroethylene cross-linked composite carbon cathode mixture by anhydrous ethanol, so that the flexible supported nickel phthalocyanine composite carbon electrode prepared by the roller pressing method has good flexibility and volume effect, which is helpful for Cl 2 adsorption and conversion, reducing Cl 2 The potential dangers of causing the volume of the electrode to expand; in addition, flexible electrodes are suitable for various bending and folding shape changes, and can be used as core components of devices such as smart watches, bracelets, and smart glasses. Compared with rigid electrodes, they have a wider range of applications.

[0025] The flexible supported nickel phthalocyanine composite carbon electrode prepared by the roller pressing method has the characteristics of simple preparation method, good stability, good uniformity, high yield, low energy consumption and good repeatability, and can effectively add the catalyst evenly to the carbon electrode, thereby improving the SOCl 2 and Cl 2 The conversion efficiency is improved, and the charge and discharge performance of the battery is improved. Compared with the rechargeable lithium / thionyl chloride battery assembled with pure acetylene black as the electrode, the average coulombic efficiency of the rechargeable lithium / thionyl chloride battery assembled with flexible supported nickel phthalocyanine composite carbon electrode is increased by about 15%, and it has a longer and more stable cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 : Rechargeable Li / SOCl assembled with the flexible supported nickel phthalocyanine composite carbon electrode prepared in Example 1 of the present invention 2 Battery cycle performance diagram;

[0027] Figure 2 : Rechargeable Li / SOCl assembled with the flexible supported nickel phthalocyanine composite carbon electrode prepared in Example 1 of the present invention 2 Battery rate performance diagram;

[0028] Figure 3 : Rechargeable Li / SOCl assembled with the flexible supported nickel phthalocyanine composite carbon electrode prepared in Example 1 of the present invention 2 Battery charge and discharge curves;

[0029] Figure 4 : SEM image of the activated carbon-supported nickel phthalocyanine composite material prepared in Example 1 of the present invention;

[0030] Figure 5 : FT-IR image of the activated carbon-supported nickel phthalocyanine composite material prepared in Example 1 of the present invention;

[0031] Figure 6 : Raman image of the activated carbon-supported nickel phthalocyanine composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.

[0033] Example 1

[0034] Step 1, 0.1 g of pyroasphalt activated carbon, 0.82 g of phthalic anhydride, 1.2 g of urea, 0.61 g of nickel chloride hexahydrate and 0.12 g of ammonium molybdate tetrahydrate were mixed and ground to obtain a mixture A;

[0035] Step 2, putting mixture A into a crucible and placing it in a muffle furnace, under an air atmosphere, heating from room temperature to 140°C at a heating rate of 10°C / min and keeping warm for 0.5h, then heating to 270°C at a heating rate of 10°C / min, keeping warm for 2h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for 12h, removing the upper suspended matter first, then soaking in water again, repeating 3 times, then washing with anhydrous ethanol 3 times, then washing with deionized water 3 times, and then drying at 105°C for 12h to obtain an activated carbon-supported nickel phthalocyanine composite material, recorded as NiPc / AC;

[0036] Step 3, 0.0213 g of a polytetrafluoroethylene emulsion having a solid content of 60% was mixed with 1.167 g of deionized water, and stirred for 30 minutes to obtain a polytetrafluoroethylene emulsion dilution;

[0037] Step 4, acetylene black and NiPc / AC are put into a mortar according to a mass ratio of 100:6, and stirred evenly to obtain a mixture B. According to the mass ratio of the mixture B to the polytetrafluoroethylene emulsion diluent of 1:4.7, the polytetrafluoroethylene emulsion diluent is added to the mortar containing the mixture B, and then a trace amount of anhydrous ethanol is added. After grinding into a uniform mass, the mixture is transferred to a crucible, and the crucible is placed in a muffle furnace. The temperature is raised from room temperature to 180°C at a heating rate of 10°C / min, and the mixture is dried for 24 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;

[0038] Step 5, first soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 20 minutes, take it out and wrap it with plastic wrap, use a roller press to squeeze out the anhydrous ethanol at a small pressure, then cut it, and then remove the plastic wrap, and press it with working thicknesses of 1.75mm, 1.25mm, 0.75mm and 0.25mm in turn, and finally dry it at 60°C for 24h, remove the anhydrous ethanol, and obtain a flexible supported nickel phthalocyanine composite carbon electrode with a thickness of 0.25mm.

[0039] Figure 4 This is a SEM image of the activated carbon-supported nickel phthalocyanine composite material NiPc / AC prepared in Example 1. It can be seen from the figure that after the addition of activated carbon, the catalytic material produces a lot of pore structures, and these pores can make LiCl and S better converted and utilized during the charge and discharge process.

[0040] Figure 5 and Figure 6 They are FT-IR and Raman images of the activated carbon-supported nickel phthalocyanine composite material NiPc / AC prepared in Example 1 of the present invention. It can be seen that the activated carbon-supported nickel phthalocyanine composite material NiPc / AC was successfully prepared in Example 1.

[0041] The flexible supported nickel phthalocyanine composite carbon electrode prepared in Example 1 was punched with a punching machine, cut into pieces, and assembled into a rechargeable lithium / thionyl chloride battery. The electrochemical performance test was carried out. The results are as follows: Figure 1 to Figure 3 As shown:

[0042] Figure 1 This is the cycle performance diagram of the rechargeable lithium / thionyl chloride battery. It can be seen that after the activated carbon-loaded nickel phthalocyanine composite material is introduced into the carbon electrode, the rechargeable lithium / thionyl chloride battery can be cycled about 100 times, and the coulombic efficiency is always maintained at about 98%, and the specific capacity can reach 1200mAh / g.

[0043] Figure 2 This is the rate performance diagram of the rechargeable lithium / thionyl chloride battery. It can be seen that at different discharge current densities, the rechargeable lithium / thionyl chloride battery can maintain good coulombic efficiency and specific capacity.

[0044] Figure 3 Figure 3 is the charge and discharge curve of the rechargeable lithium / thionyl chloride battery. It can be seen that after the activated carbon-loaded nickel phthalocyanine composite material is introduced into the carbon electrode, the charging and discharging platforms of the rechargeable lithium / thionyl chloride battery are relatively stable.

[0045] Example 2

[0046] Step 1, 0.21 g of pyroasphalt activated carbon, 0.71 g of phthalic anhydride, 1.42 g of urea, 0.58 g of nickel chloride hexahydrate and 0.13 g of ammonium molybdate tetrahydrate were mixed and ground to obtain a mixture A;

[0047] Step 2, putting mixture A into a crucible and placing it in a muffle furnace, under an air atmosphere, heating from room temperature to 130°C at a heating rate of 5°C / min and keeping warm for 1h, then heating to 280°C at a heating rate of 5°C / min, keeping warm for 3h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for 12h, removing the upper suspended matter first, then soaking in water again, repeating 3 times, then washing with anhydrous ethanol 2 times, then washing with deionized water once, and then drying at 60°C for 24h to obtain an activated carbon-supported nickel phthalocyanine composite material, recorded as NiPc / AC;

[0048] Step 3, 0.03 g of a polytetrafluoroethylene emulsion having a solid content of 60% was mixed with 1.4 g of deionized water, and stirred for 30 min to obtain a polytetrafluoroethylene emulsion dilution;

[0049] Step 4, according to the mass ratio of 100:5, acetylene black and NiPc / AC are put into a mortar, stirred evenly to obtain a mixture B, and the polytetrafluoroethylene emulsion diluent is added to the mortar containing the mixture B according to the mass ratio of the mixture B to the polytetrafluoroethylene emulsion diluent of 1:4.7, and then a trace amount of anhydrous ethanol is added, and after grinding into a uniform mass, the crucible is transferred to a crucible, and the crucible is placed in a muffle furnace, and the temperature is increased from room temperature to 190°C at a heating rate of 5°C / min, and dried for 20 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;

[0050] Step 5, first soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 6 hours, take it out and wrap it with plastic wrap, use a roller press to extrude the anhydrous ethanol with a small pressure, then cut it, and then remove the plastic wrap, and press it with working thicknesses of 2mm, 1.5mm, 1.0mm and 0.75mm in turn, and finally dry it at 100°C for 12h, remove the anhydrous ethanol, and obtain a flexible supported nickel phthalocyanine composite carbon electrode with a thickness of 0.75mm.

[0051] Example 3

[0052] Step 1, 0.25 g of pyroasphalt activated carbon, 0.78 g of phthalic anhydride, 1.38 g of urea, 0.67 g of nickel chloride hexahydrate and 0.17 g of ammonium molybdate tetrahydrate were mixed and ground to obtain a mixture A;

[0053] Step 2, putting mixture A into a crucible and placing it in a muffle furnace, under an air atmosphere, heating from room temperature to 130°C at a heating rate of 8°C / min and keeping warm for 2h, then heating to 290°C at a heating rate of 8°C / min, keeping warm for 1h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for 12h, removing the upper suspended matter, then soaking in water, repeating 3 times, washing with anhydrous ethanol 4 times, then washing with deionized water 2 times, and then drying at 120°C for 18h to obtain an activated carbon-supported nickel phthalocyanine composite material, recorded as NiPc / AC;

[0054] Step 3, 0.025 g of a polytetrafluoroethylene emulsion having a solid content of 60% was mixed with 1.2 g of deionized water, and stirred for 30 min to obtain a polytetrafluoroethylene emulsion dilution;

[0055] Step 4, according to the mass ratio of 100:4, acetylene black and NiPc / AC are put into a mortar, stirred evenly to obtain a mixture B, and the polytetrafluoroethylene emulsion diluent is added to the mortar containing the mixture B according to the mass ratio of the mixture B to the polytetrafluoroethylene emulsion diluent of 1:4.7, and then a trace amount of anhydrous ethanol is added, and after grinding into a uniform mass, the crucible is transferred to a crucible, and the crucible is placed in a muffle furnace, and the temperature is increased from room temperature to 200°C at a heating rate of 8°C / min, and dried for 10 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;

[0056] Step 5, first soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 12 hours, take it out and wrap it with plastic wrap, use a roller press to squeeze out the anhydrous ethanol at a small pressure, then cut it, and then remove the plastic wrap, and press it with working thicknesses of 2mm, 1.5mm, 1.0mm and 0.75mm in turn, and finally dry it at 50°C for 18h, remove the anhydrous ethanol, and obtain a flexible supported nickel phthalocyanine composite carbon electrode with a thickness of 0.75mm.

[0057] Example 4

[0058] Step 1, 0.3 g of pyroasphalt activated carbon, 0.85 g of phthalic anhydride, 1.68 g of urea, 0.88 g of nickel chloride hexahydrate and 0.21 g of ammonium molybdate tetrahydrate were mixed and ground to obtain a mixture A;

[0059] Step 2, putting mixture A into a crucible and placing it in a muffle furnace, in an air atmosphere, heating from room temperature to 150°C at a heating rate of 10°C / min and keeping warm for 1.5 hours, then heating to 290°C at a heating rate of 10°C / min, keeping warm for 2 hours, and cooling naturally to room temperature. After grinding into powder, soaking in deionized water for 12 hours, first removing the upper suspended matter, then soaking in water, repeating 3 times, then washing with anhydrous ethanol 3 times, then washing with deionized water 4 times, and then drying at 100°C for 12 hours to obtain an activated carbon-supported nickel phthalocyanine composite material, recorded as NiPc / AC;

[0060] Step 3, 0.02 g of a polytetrafluoroethylene emulsion having a solid content of 60% was mixed with 1.3 g of deionized water, and stirred for 30 min to obtain a polytetrafluoroethylene emulsion dilution;

[0061] Step 4, acetylene black and NiPc / AC are put into a mortar according to a mass ratio of 100:7, and stirred evenly to obtain a mixture B. According to the mass ratio of the mixture B to the polytetrafluoroethylene emulsion diluent of 1:4.7, the polytetrafluoroethylene emulsion diluent is added to the mortar containing the mixture B, and then a trace amount of anhydrous ethanol is added. After grinding into a uniform mass, the mixture is transferred to a crucible, and the crucible is placed in a muffle furnace. The temperature is raised from room temperature to 170°C at a heating rate of 10°C / min, and the mixture is dried for 4 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;

[0062] Step 5, first soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 18 hours, take it out and wrap it with plastic wrap, use a roller press to squeeze out the anhydrous ethanol at a small pressure, then cut it, and then remove the plastic wrap, press it with working thicknesses of 1.75mm, 1.25mm, 0.75mm and 0.25mm in turn, and finally dry it at 80°C for 6 hours to remove the anhydrous ethanol to obtain a flexible supported nickel phthalocyanine composite carbon electrode with a thickness of 0.25mm.

[0063] Example 5

[0064] Step 1, 0.15 g of pyroasphalt activated carbon, 0.68 g of phthalic anhydride, 1.08 g of urea, 0.45 g of nickel chloride hexahydrate and 0.2 g of ammonium molybdate tetrahydrate were mixed and ground to obtain a mixture A;

[0065] Step 2, putting mixture A into a crucible and placing it in a muffle furnace, under an air atmosphere, heating from room temperature to 160°C at a heating rate of 8°C / min and keeping warm for 0.5h, then heating to 260°C at a heating rate of 8°C / min, keeping warm for 3h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for 12h, removing the upper suspended matter first, then soaking in water again, repeating 3 times, then washing with anhydrous ethanol 3 times, then washing with deionized water 5 times, and then drying at 80°C for 20h to obtain an activated carbon-supported nickel phthalocyanine composite material, recorded as NiPc / AC;

[0066] Step 3, 0.03 g of a polytetrafluoroethylene emulsion having a solid content of 60% was mixed with 1.5 g of deionized water, and stirred for 30 min to obtain a polytetrafluoroethylene emulsion dilution;

[0067] Step 4, acetylene black and NiPc / AC are put into a mortar according to a mass ratio of 100:8, and stirred evenly to obtain a mixture B. According to the mass ratio of the mixture B to the polytetrafluoroethylene emulsion diluent of 1:4.7, the polytetrafluoroethylene emulsion diluent is added to the mortar containing the mixture B, and then a trace amount of anhydrous ethanol is added. After grinding into a uniform mass, the mixture is transferred to a crucible, and the crucible is placed in a muffle furnace. The temperature is raised from room temperature to 160°C at a heating rate of 5°C / min, and the mixture is dried for 15 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;

[0068] Step 5, first soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 24 hours, take it out and wrap it with plastic wrap, use a roller press to squeeze out the anhydrous ethanol at a small pressure, then cut it, and then remove the plastic wrap, and press it with working thicknesses of 2mm, 1.5mm, 1.0mm and 0.5mm in turn, and finally dry it at 130°C for 2h, remove the anhydrous ethanol, and obtain a flexible supported nickel phthalocyanine composite carbon electrode with a thickness of 0.5mm.

Claims

1. A method for preparing a flexible supported nickel phthalocyanine composite carbon electrode, characterized in that: The steps include: Step 1, mixing and grinding pyroasphalt activated carbon, phthalic anhydride, urea, nickel chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of (0.1-0.3):(0.68-0.85):(1.08-1.68):(0.45-0.88):(0.12-0.21) to obtain a mixture A; Step 2, placing the mixture A into a muffle furnace, heating the mixture from room temperature to 130-160° C. at a heating rate of 5-10° C. / min in an air atmosphere and keeping the temperature for 0.5-2 h, then heating the mixture to 260-290° C. at a heating rate of 5-10° C. / min, keeping the temperature for 1-3 h, cooling the mixture naturally to room temperature, grinding, soaking, washing and drying the mixture in turn to obtain an activated carbon-supported nickel phthalocyanine composite material; Step 3, mixing a polytetrafluoroethylene emulsion having a solid content of 60% with deionized water in a mass ratio of (0.02-0.03):(1.167-1.5), stirring evenly, and obtaining a polytetrafluoroethylene emulsion dilution; Step 4, acetylene black and activated carbon-supported nickel phthalocyanine composite material are mixed in a mass ratio of 100:(4-8), stirred evenly to obtain a mixture B, and the mixture B is added to a polytetrafluoroethylene emulsion diluent in a mass ratio of 1:4.7, and then a trace amount of anhydrous ethanol is added, ground evenly, and then dried to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture; Step 5: After soaking the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol, the mixture is gradually rolled and dried using a roller press to obtain a flexible supported nickel phthalocyanine composite carbon electrode.

2. The method for preparing the flexible supported nickel phthalocyanine composite carbon electrode according to claim 1, characterized in that: The soaking in step 2 is to soak in deionized water for at least 12 hours, remove the upper suspended matter, then change the water for soaking, and repeat 3 times.

3. The method for preparing the flexible supported nickel phthalocyanine composite carbon electrode according to claim 1, characterized in that: The cleaning in step 2 is firstly cleaning with anhydrous ethanol for 2 to 4 times, and then cleaning with deionized water for 1 to 5 times.

4. The method for preparing the flexible supported nickel phthalocyanine composite carbon electrode according to claim 1, characterized in that: The drying in step 2 is performed at 60 to 150° C. for 12 to 24 hours.

5. The method for preparing the flexible supported nickel phthalocyanine composite carbon electrode according to claim 1, characterized in that: The drying in step 4 is performed by using a muffle furnace or an oven, heating the temperature from room temperature to 160-200° C. at a heating rate of 5-10° C. / min, and drying for 4-24 hours.

6. The method for preparing the flexible supported nickel phthalocyanine composite carbon electrode according to claim 1, characterized in that: In step 5, the polytetrafluoroethylene cross-linked composite carbon cathode mixture is immersed in anhydrous ethanol for 20 minutes to 24 hours.

7. The method for preparing the flexible supported nickel phthalocyanine composite carbon electrode according to claim 1, characterized in that: The process of step 5 of gradually rolling the electrode using a roller press is as follows: first, anhydrous ethanol is extruded using a roller press at a small pressure, then cut, and then pressed in sequence with working thicknesses of 1.75-2 mm, 1.25-1.5 mm, 0.75-1.0 mm, and 0.25-0.75 mm to obtain a flexible supported nickel phthalocyanine composite carbon electrode with a thickness of 0.25-0.75 mm.

8. The method for preparing the flexible supported nickel phthalocyanine composite carbon electrode according to claim 1, characterized in that: The drying in step 5 is carried out at 50-130° C. for 2-24 hours.

9. A flexible supported nickel phthalocyanine composite carbon electrode prepared by the method according to any one of claims 1 to 8.

10. Use of the flexible supported nickel phthalocyanine composite carbon electrode according to claim 9 as a positive electrode of a rechargeable lithium / thionyl chloride battery.