Sodium-ion battery negative electrode material, sodium-ion battery and preparation method of sodium-ion battery negative electrode material
By using Ti3Sn5S12/rGO material in sodium ion batteries, combining the reduction of graphene oxide and titanium elements, the problem of volume expansion and insufficient conductivity of the negative electrode material of sodium ion batteries during charging and discharging is solved, and the stability and performance of the material are improved .
Patent Information
- Application Number
- CN202410988601.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing sodium ion battery anode materials have severe expansion/contraction and insufficient conductivity during charging and discharging, which limits their practical application.
Ti3Sn5S12/rGO is used as the negative electrode material of sodium ion battery. By introducing reducing graphene oxide and titanium elements, the volume expansion effect is alleviated and the conductivity is improved. The preparation method includes high-temperature synthesis and ball milling treatment.
It significantly reduces the volume expansion of the negative electrode material of sodium ion battery, improves conductivity and cycling stability, and enhances electrochemical performance.
Smart Images

Figure CN118943323A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and specifically to sodium ion battery negative electrode materials, sodium ion batteries and preparation methods thereof. Background Art
[0002] Sodium-ion batteries are currently receiving increasing attention. Sulfides have become competitive negative electrode materials for building sodium-ion batteries due to their advantages of high ionic conductivity and good rate performance. However, the essential defects of binary sulfides, such as severe expansion / contraction during charging and discharging and the conductivity that still needs to be improved, hinder their practical application. Therefore, the negative electrode materials of sodium-ion batteries still need to be improved. Summary of the invention
[0003] The embodiments of the present application provide a sodium ion battery negative electrode material, a sodium ion battery and a preparation method thereof, so that when the improved sodium ion battery negative electrode material is used during the charge and discharge process, the volume expansion effect of the sodium ion battery negative electrode material is weakened and the conductivity can be improved.
[0004] The present invention provides a method for preparing a negative electrode material for a sodium ion battery, comprising the following steps:
[0005] Adding titanium tetrachloride, tin dichloride dihydrate and thiourea in sequence into a stainless steel autoclave lined with polytetrafluoroethylene, and adding anhydrous ethanol into the stainless steel autoclave to obtain a first mixture;
[0006] After stirring the first mixture, a second mixture is obtained;
[0007] Sealing the stainless steel autoclave containing the second mixture, and placing the sealed stainless steel autoclave in a preset first high temperature environment for a first preset time period;
[0008] Obtaining a first product after high temperature treatment from a stainless steel autoclave placed in a preset first high temperature environment for a first preset period of time;
[0009] Washing the first product to obtain a second product;
[0010] placing the second product under a preset second suitable temperature environment for a second preset period of time for drying to obtain a titanium tin sulfur product;
[0011] mixing the titanium tin sulfur product with reduced graphene oxide to obtain a third mixture;
[0012] Grinding the third mixture to obtain a fourth mixture;
[0013] The fourth mixture is ball-milled to obtain a fifth mixture, which is used as a negative electrode material for a sodium ion battery.
[0014] The present invention provides a method for manufacturing a sodium ion battery, comprising the following steps:
[0015] Grinding a sodium ion battery negative electrode material, a conductive agent and a binder to obtain a sixth mixture, wherein the sodium ion battery negative electrode material is a sodium ion battery negative electrode material prepared according to the above-mentioned method for preparing a sodium ion battery negative electrode material;
[0016] Taking deionized water as a solvent, mixing the sixth mixture with the deionized water to obtain a slurry;
[0017] Stirring the slurry, and applying the stirred slurry on the copper foil;
[0018] After the surface of the copper foil coated with the stirred slurry is air-dried, the copper foil after the surface is air-dried is subjected to drying treatment to obtain the dried copper foil as the negative electrode sheet of the sodium ion battery;
[0019] Using glass fiber as the diaphragm material of the sodium ion battery and using the sodium sheet as the counter electrode and reference electrode of the sodium ion battery;
[0020] A sodium ion battery is obtained according to the negative electrode sheet, the separator material, the counter electrode and the reference electrode.
[0021] An embodiment of the present application provides a sodium ion battery, wherein the negative electrode material of the sodium ion battery is the negative electrode material of the sodium ion battery in the above embodiment.
[0022] Compared with the prior art, the embodiments of the present application have the following advantages: reduced graphene oxide is introduced in the embodiments of the present application for preparing the negative electrode material of the sodium ion battery. Since the density of reduced graphene oxide is very low and the gap structure is very stable and tight, the deformation of the lattice and the expansion of the negative electrode material of the sodium ion battery can be prevented, thereby improving the stability of the negative electrode material of the sodium ion battery. In addition, the sodium inert element titanium is also introduced in the embodiments of the present application, which can not only improve the conductivity of the sodium ion battery, but also alleviate the volume expansion of the negative electrode material of the sodium ion battery during the charging and discharging process to a certain extent, thereby improving the stability of the sodium ion battery during the charging and discharging process. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a flow chart of a method for preparing a negative electrode material for a sodium ion battery provided in the first embodiment of the present application;
[0024] Figure 2 It is Ti3Sn5S provided in the first embodiment of the present application. 12 / rGO and Ti3Sn5S 12 0.2Ag -1 Cycle capacity diagram;
[0025] Figure 3 It is Ti3Sn5S provided in the first embodiment of the present application. 12 / rGO and Ti3Sn5S 12 Electrochemical impedance spectroscopy of
[0026] Figure 4 is a flow chart of a method for preparing a sodium ion battery provided in the third embodiment of the present application;
[0027] Figure 5 is a flow chart of a method for preparing a negative electrode material for a sodium ion battery provided in the tenth embodiment of the present application;
[0028] Figure 6 is the XRD diagram of Cu3SnS4 / rGO and Cu3SnS4 provided in the tenth embodiment of the present application;
[0029] Figure 7 The 0.2Ag of Cu3SnS4 / rGO and Cu3SnS4 provided in the tenth embodiment of the present application -1 Cycle capacity diagram;
[0030] Figure 8 is the electrochemical impedance spectrum of Cu3SnS4 / rGO and Cu3SnS4 provided in the tenth embodiment of the present application;
[0031] Fig. 9 This is a flow chart of a method for preparing a sodium ion battery provided in the twelfth embodiment of the present application. DETAILED DESCRIPTION
[0032] Many specific details are described in the following description to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present application, so the present application is not limited by the specific implementation disclosed below.
[0033] Lithium-ion batteries (LIBs) have been rapidly and widely used in electric vehicles and portable electronic devices. However, limited exploitable lithium resources cannot guarantee sustainable consumption. In recent years, sodium-ion batteries (SIBs) have attracted increasing attention due to their abundant sodium resources and similar physical and chemical properties to lithium-ion batteries. Various electrolytes and cathode materials for sodium-ion batteries have been proposed in a large number of studies. However, the large ionic size of sodium ions leads to slow sodium kinetics and huge volume changes in negative electrode materials, which is not conducive to the development of high-performance sodium-ion batteries. Therefore, it is imperative to rationally design negative electrode materials for sodium-ion batteries with superior comprehensive performance. In the prior art, sulfides have the advantages of high ionic conductivity and good rate performance compared with negative electrode materials made of oxides, making them a competitive negative electrode material for constructing sodium-ion batteries. However, the essential defects of binary sulfides, such as severe expansion / contraction during charging and discharging and conductivity that still needs to be improved, hinder their practical application. Therefore, the negative electrode materials of sodium-ion batteries still need to be improved.
[0034] As a typical alloy-type negative electrode material, tin-based compounds have become the first choice for SIBs negative electrode materials due to their high specific capacity. In order to further optimize the sodium storage performance of tin-based sulfides, technicians in this field have studied the possibility of using ternary tin-based compounds to prepare negative electrode materials for sodium-ion batteries.
[0035] After research, the applicant believes that Ti3Sn5S 12 As a ternary tin-based compound, it has multiple advantages. First, it has a high theoretical specific capacity (mAh g -1 Specific capacity is an important parameter to measure the performance of battery electrode materials. It indicates the amount of charge that the electrode material can store per unit mass. It is usually expressed in milliampere-hours per gram (mAh / g) or ampere-hours per kilogram (Ah / kg). mAh is milliampere-hour, which is the unit of electricity and indicates the amount of electricity that can be provided by continuous discharge at a current of milliamperes (mA) for one hour. -1 It stands for per gram, which means unit mass. Combining these two units, mAh g -1 mAh / g refers to the amount of electricity that can be provided per gram of electrode material. This parameter is crucial for evaluating battery performance because it is directly related to the battery's energy density and cycle stability. For example, if an electrode material has a high mAhg -1 Theoretical specific capacity refers to the maximum amount of charge that a material can store per gram of material under ideal conditions. 12 The theoretical specific capacity is 1021.3 mAh g -1 , which means that theoretically, per gram of Ti3Sn5S12 It can store 1021.3 mAh of charge. This is a relatively high value, indicating that Ti3Sn5S 12 It has a large sodium storage capacity. 12 The sodium inactive element titanium (Ti) is contained in the battery. The introduction of titanium can alleviate the volume effect of the negative electrode material of the battery during the charge and discharge process to a certain extent, thereby improving the electrochemical performance of the battery. The applicant found that compared with the theoretical specific capacity, the bare Ti3Sn5S 12 In actual applications, the particles show insufficient reversible capacity and fast capacity decay. Reversible capacity refers to the capacity that can actually be used in the battery during the charge and discharge cycle, and capacity decay refers to the gradual decrease in the battery's ability to store electrical energy after multiple charge and discharge processes. 12 The defects of the particles in practical applications, the applicant also found after research that reduced graphene oxide (rGO, Reduced Graphene Oxider) has excellent conductivity and mechanical properties, and is a negative electrode additive that helps to alleviate the volume change of the negative electrode material during charging and discharging and improve the electrochemical performance. Therefore, the preparation of ternary tin-based sulfides anchored on reduced graphene oxide can obtain high reversible capacity and good cycle stability.
[0036] Based on the above analysis, the present embodiment adopts Ti3Sn5S 12 / rGO is used as the negative electrode material of sodium ion battery. When preparing the negative electrode material of sodium ion battery, Ti3Sn5S can be synthesized by solvothermal method. 12 , and then Ti3Sn5S was prepared by ball milling 12 / rGO composite material. This composite material can buffer the volume expansion of the negative electrode material of the sodium ion battery during the charging and discharging process and promote the rapid transfer of electrons.
[0037] Various embodiments of the present application are described below in conjunction with the accompanying drawings.
[0038] The first embodiment of the present application provides a method for preparing a negative electrode material for a sodium ion battery. Figure 1 The flow chart of the preparation method of the negative electrode material of the sodium ion battery provided in the first embodiment of the present application is as follows: Figure 1 The method provided in this embodiment is described in detail. The embodiments described below are used to explain the principle of the method and are not intended to be limiting for actual use.
[0039] like Figure 1 As shown, the method for preparing the negative electrode material of a sodium ion battery provided in this embodiment comprises the following steps:
[0040] S101, titanium tetrachloride, tin dichloride dihydrate and thiourea are added to a stainless steel autoclave lined with polytetrafluoroethylene in sequence, and anhydrous ethanol is added to the stainless steel autoclave to obtain a first mixture. Specifically, 0.189g of titanium tetrachloride (TiCl4), 0.376g of tin dichloride dihydrate (SnCl2·2H2O) and 0.304g of thiourea can be added to a 50ml stainless steel autoclave lined with polytetrafluoroethylene in sequence, and 45ml of anhydrous ethanol is added to the stainless steel autoclave to obtain a mixture of titanium tetrachloride, tin dichloride dihydrate, thiourea and anhydrous ethanol. For ease of description, the mixture obtained here is referred to as the first mixture. Titanium tetrachloride (TiCl4), as a titanium source, provides titanium element (Ti) during the preparation process. Introducing titanium element into battery materials has the following advantages: First, titanium (Ti) is a metal with a relatively high elastic modulus. The elastic modulus represents the ability of a material to resist deformation, usually in Pascals (Pa) or GPa. The elastic modulus of titanium is about 110GPa, which is higher than many other metals and alloys. For example, the elastic modulus of aluminum is about 70GPa, and the elastic modulus of titanium is at a relatively high level among metal materials. A high elastic modulus means that the deformation per unit length of the material is smaller when it is subjected to force, that is, the material is harder and not easily compressed or stretched. When subjected to the same force, the deformation of the material with a high elastic modulus will be relatively small. During the battery charging and discharging process, there is a volume effect, which refers to the volume change of the positive and negative electrode materials due to the embedding and de-embedding of ions. This volume change may cause structural damage to the material, thereby affecting the cycle stability of the battery. The introduction of titanium can alleviate this volume effect to a certain extent. Titanium has a higher elastic modulus, which means that it deforms less when subjected to force, which helps to maintain the structural stability of the battery material, thereby alleviating this volume effect.
[0041] Secondly, during the battery charging and discharging process, volume changes may lead to stress concentration. Stress is a physical quantity that describes the material's resistance to deformation. When external force acts on an object, internal forces will be generated inside the object. The distribution of these internal forces on the cross section of the object is called stress. Stress concentration means that during the charging and discharging process, stress may be concentrated in certain areas of the battery material, especially between particles or microcracks, resulting in stress at these locations much higher than other areas. Continuous stress can easily lead to the formation and expansion of microcracks in the battery material, and eventually lead to particle rupture. Over time, particle rupture can cause the electrode material to pulverize, reduce the conductivity of the electrode, increase the internal resistance of the battery, and affect the battery performance. The addition of titanium can serve as a supporting structure to help disperse the stress caused by ion embedding and extraction, thereby reducing the rupture and pulverization of the material and improving the overall performance and life of the battery. The addition of titanium can also improve the toughness of the battery material, making it more able to withstand volume changes during charging and discharging, and reducing the generation and spread of cracks. In addition, titanium has good chemical stability and is not prone to adverse reactions with other components in the battery, which helps to improve the cycle stability of the battery material. In addition, titanium also has thermal stability, which refers to the ability of titanium to maintain its chemical and physical properties unchanged in high temperature environments. Specifically, titanium has good creep resistance at high temperatures, which means that it deforms less under continuous stress and can maintain structural stability. Titanium has a relatively low coefficient of thermal expansion, which makes its volume change less when the temperature changes, which helps maintain the dimensional stability of the material. Titanium also has moderate thermal conductivity, which helps to quickly transfer heat in applications that require heat dissipation. Due to these thermal stability characteristics, titanium helps the battery maintain temperature stability during charging and discharging, reducing material performance degradation caused by temperature changes.
[0042] In summary, the addition of titanium can alleviate the volume effect of battery materials and improve the performance and life of the battery through various mechanisms.
[0043] Tin dichloride dihydrate (SnCl2·2H2O) is used as a tin source to provide tin element (Sn) during the reaction. Tin element is one of the key materials for forming ternary tin-based compounds. Tin has a high theoretical specific capacity, which means that under the same mass conditions, tin-based negative electrode materials can store more charge. Tin can also form alloys with sodium. The alloying ability of tin enables it to absorb and release a large amount of sodium ions during the charge and discharge process. This process usually involves a multi-electron transfer process, which increases the amount of charge that each tin atom can store, thereby improving the energy density of the material.
[0044] Thiourea is a sulfur-containing compound that can participate in the reaction as a sulfur source to help form sulfide materials. In addition, thiourea can also act as a reducing agent in certain circumstances, helping to lower the reaction temperature or promote the progress of a specific chemical reaction.
[0045] PTFE is used as a lining for stainless steel autoclaves. Due to its excellent corrosion resistance and non-reactivity, PTFE can protect the reaction vessel from being attacked by corrosive chemicals, and also prevent the reactants from having undesirable chemical reactions with the container. At the same time, the PTFE lining can provide a smooth contact surface, which helps to improve the stirring efficiency and ensure that the reactants are evenly mixed during the reaction process. It can also prevent cross-contamination between different batches of reactions because PTFE does not adsorb reactants or products. PTFE lining is easy to clean, which helps to reduce losses during the cleaning process and maintain the cleanliness of the reaction vessel. PTFE also has good high temperature resistance and can remain stable at high temperatures of 200°C, which makes it suitable for use in high-temperature synthesis processes. By using a stainless steel autoclave lined with PTFE, the smooth progress of the synthesis process can be ensured, while improving the quality and purity of the product.
[0046] Anhydrous ethanol as a solvent helps to form a uniform slurry, which is equivalent to providing a uniform reaction environment, which helps to fully contact and react between the reactants, thereby improving the reaction efficiency.
[0047] Please refer to Figure 1 , after executing S101, executing S102, that is, after stirring the first mixture, a second mixture is obtained. Specifically, the first mixture can be stirred for 10 minutes, and stirring can make all reactants fully contact and prevent the reactants from being excessively concentrated in a local area. For ease of description, the mixture obtained after stirring is referred to as the second mixture. That is, as an embodiment, the first mixture is stirred for 10 minutes.
[0048] After executing S102, execute S103, that is, seal the stainless steel autoclave containing the second mixture, and place the sealed stainless steel autoclave in a preset first high temperature environment for a first preset time. Specifically, the stainless steel autoclave containing the second mixture can be sealed at 200°C for 12 hours, and the reaction can be completed. That is, as an embodiment, the preset first high temperature environment can refer to an environment of 200°C, and the first preset time can refer to 12 hours.
[0049] S104, obtaining a first product after high temperature treatment from a stainless steel autoclave placed in a preset first high temperature environment for a first preset time. Specifically, after the stainless steel autoclave containing the second mixture is sealed and maintained at 200° C. for 12 hours, a product after high temperature treatment can be obtained from the stainless steel autoclave. As an embodiment, the first product can be a black fluffy product filtered out from the stainless steel autoclave.
[0050] S105, washing the first product to obtain a second product. Specifically, the first product can be washed several times with ethanol and distilled water to obtain the second product. As an embodiment, ethanol and distilled water can be used to remove the solvent and other soluble impurities remaining on the surface of the black fluffy product to obtain a washed black fluffy product, and the washed black fluffy product is the second product.
[0051] S106, placing the second product in a preset second suitable temperature environment for a second preset time, and drying it to obtain a titanium tin sulfur product. Specifically, the washed black fluffy product is placed in a 60°C environment and vacuum dried for 4 hours to obtain Ti3Sn5S 12 Solid, the Ti3Sn5S 12 The solid is a titanium tin sulfur product. That is, as an embodiment, the second suitable temperature environment may be an environment of 60° C., the second preset time may be 4 hours, and the drying process is performed in a vacuum environment.
[0052] S107, mixing the titanium tin sulfur product with reduced graphene oxide to obtain a third mixture. Specifically, the titanium tin sulfur product and reduced graphene oxide can be mixed at a mass ratio of 4:1. For example, 0.1 g of Ti3Sn5S 12 Mixed with 0.025 g of rGO to obtain Ti3Sn5S 12 That is, as an example, the titanium tin sulfur product and reduced graphene oxide can be mixed at a mass ratio of 4:1 to obtain a mixture of the titanium tin sulfur product and reduced graphene oxide. For ease of description, the mixture obtained here is referred to as a third mixture.
[0053] S108, grinding the third mixture to obtain a fourth mixture. 12 The mixture with rGO is ground evenly. For the convenience of description, the ground Ti3Sn5S 12 The mixture with rGO is called the fourth mixture.
[0054] S109, ball milling the fourth mixture to obtain a fifth mixture as a negative electrode material for a sodium ion battery. 12 The mixture with rGO was placed in a planetary ball mill and ball milled at 400 rpm for 8 h to obtain Ti3Sn5S 12 For ease of description, the milled Ti3Sn5S 12The mixture with rGO is called the fifth mixture. The fifth mixture can be used as the negative electrode material of the sodium ion battery.
[0055] Since the first embodiment of the present application proposes to introduce rGO into the negative electrode material of the sodium ion battery, the first embodiment of the present application has the following advantages: First, rGO has excellent electronic conductivity. 12 Mixing can improve the conductivity of the overall electrode, thereby reducing the internal resistance during the battery charging and discharging process and improving battery performance. Secondly, the two-dimensional layered structure of rGO can serve as a support to enhance the structural stability of the composite material, help maintain the structural integrity of the electrode material during the charging and discharging process, and provide a certain buffer space, which helps to alleviate the problem of battery material rupture or stratification caused by volume expansion. At the same time, due to the high conductivity and mechanical stability of rGO, the breakage and shedding of electrode materials during the cycle can be reduced, extending the service life of the battery. The channels present in the rGO layered structure also help the diffusion of sodium ions and improve the ion transport performance of the material, thereby increasing the charge and discharge rate of the battery. In addition, rGO also has a high specific surface area, which helps to increase the contact area between the electrode and the electrolyte, thereby increasing the reaction activity of the electrode. These factors work together to help achieve the development of high-performance sodium-ion batteries.
[0056] The sodium ion battery negative electrode material prepared in the first embodiment of the present application is specifically Ti3Sn5S 12 / rGO, Ti3Sn5S 12 / rGO is compounded with rGO. Since the density of rGO is very low and the gap structure is very stable and tight, the deformation of the lattice and the expansion of the negative electrode material of the sodium ion battery can be prevented, thereby improving the stability of the negative electrode material of the sodium ion battery. In addition, the sodium inert element titanium is also introduced in the embodiment of the present application, which can not only improve the conductivity of the sodium ion battery, but also alleviate the volume expansion of the negative electrode material of the sodium ion battery during the charging and discharging process of the sodium ion battery to a certain extent, thereby improving the stability of the sodium ion battery during the charging and discharging process. In some embodiments, the above-mentioned composite rGO can also be replaced by carbon nanotubes, carbon nanofibers, Mxene, nitrogen-doped carbon, hollow carbon spheres, hard carbon, and soft carbon.
[0057] In addition, Ti3Sn5S can also be calculated according to the following chemical reaction equation 12 Theoretical specific capacity:
[0058]
[0059] According to the reaction mechanism in the above chemical reaction equation, 1 mol Ti3Sn5S 12There are 42.75 mol of electrons transferred in the reaction with sodium ions. According to the theoretical capacity calculation formula: 96485*n / (M*3.6), 96485 is the Faraday constant, n is the number of moles of electrons transferred during the electrochemical reaction, which is 42.75 in this equation, and M is the relative molecular mass of the compound, which refers to Ti3Sn5S in this equation. 12 The relative molecular mass of Ti3Sn5S 12 The relative molecular mass of Ti3Sn5S is 1121.88, from which we can get 12 The theoretical specific capacity is 1021.3 mAh g -1 .
[0060] In addition, the above equation contains an alloying reaction mechanism and a conversion reaction mechanism. The alloying reaction mechanism in this equation refers to the alloying reaction between tin and sodium ions to provide capacity, and the conversion reaction mechanism in this equation refers to the conversion reaction between sulfur and sodium ions to provide capacity, because there is electron transfer in the reaction, so it can provide capacity.
[0061] Figure 2 It is Ti3Sn5S provided in the first embodiment of the present application. 12 / rGO0.2Ag -1 Cycle capacity diagram. Figure 2 The horizontal axis represents the number of cycles, and the vertical axis represents the specific capacity. Figure 2 It is characterized that with the increase of charge and discharge cycles, Ti3Sn5S 12 / rGO and Ti3Sn5S 12 The change of specific capacity value. Among them, 0.2Ag -1 It is a parameter that represents current density, which means that in the test, the current passing through each gram of electrode material is 0.2 amperes (A). This parameter is usually used to control the current intensity during the charging and discharging process to ensure the repeatability of the experiment and the consistency of comparing the performance of different materials. Figure 2 Represents Ti3Sn5S 12 / rGO and Ti3Sn5S 12 At the same current density (0.2Ag -1 ) were used for cyclic charge and discharge tests. The lines composed of circles represent Ti3Sn5S 12 , the lines composed of pentagons represent Ti3Sn5S 12 / rGO, by Figure 2 It can be clearly seen that after several weeks of cycling, Ti3Sn5S 12 The specific capacity value is nearly 1250mAhg -1 Reduced to nearly 450mAhg -1 , reducing by almost 800mAhg -1In contrast, Ti3Sn5S 12 The specific capacity of / rGO decreased by nearly 450 mAhg -1 , it can be seen that Ti3Sn5S 12 / rGO has a higher specific capacity than Ti3Sn5S 12 , and Ti3Sn5S with rGO added 12 Compared with Ti3Sn5S12, its capacity attenuation is more alleviated. Therefore, after some cycles, the same mass of Ti3Sn5S 12 / rGO and Ti3Sn5S 12 , Ti3Sn5S 12 / rGO can provide more electrical energy, Ti3Sn5S 12 / rGO material has better performance.
[0062] Figure 3 It is Ti3Sn5S provided in the first embodiment of the present application. 12 / rGO and Ti3Sn5S 12Electrochemical impedance spectrum. Electrochemical impedance spectroscopy (EIS) is an electrochemical characterization technology. The core logic of EIS technology is to regard the electrochemical reaction as an impedance, and output impedance information at different frequencies by inputting slight disturbances. Impedance is the resistance to current changes in a circuit. It is a complex number, containing a real part (Z') and an imaginary part (Z"). The real part (Z') represents the resistive contribution, which is related to the resistance of the material, and the imaginary part (Z") represents the capacitive contribution, which is related to the capacitance of the material. For example, the impedance of a resistive element (such as a pure resistor) has only a real part and no imaginary part, and the impedance of a capacitive element (such as a pure capacitor) has only an imaginary part and no real part. In the EIS spectrum, the real part (Z') is usually used as the x-axis, and the opposite of the imaginary part (-Z") is used as the y-axis, so that the capacitive contribution can be displayed as a positive value on the EIS spectrum, thereby more intuitively reflecting the capacitive behavior. In the EIS spectrum, the larger the value of Z', the stronger the resistive contribution, and the smaller the value of Z', the weaker the resistive contribution; the larger the value of -Z", the stronger the capacitive contribution; the smaller the value of -Z", the weaker the capacitive contribution. In EIS measurement, an AC signal of known frequency and amplitude is usually applied to the sample, and then the voltage and current passing through the sample are measured. By analyzing the phase difference and amplitude between the input signal and the output response, the impedance of the sample can be calculated. The frequency axis is usually not seen directly on the EIS spectrum. Instead, the impedance is measured at multiple frequency points, and the measurement results of each frequency point will form a data point (Z', -Z"). As the frequency increases, a new data point is obtained, and the multiple data points obtained by measurement are connected into a curve displayed in the EIS spectrum. The curve shows the electrochemical behavior of the material at different frequencies. In the EIS spectrum, this curve usually appears as a semicircle or arc, and the diameter of the arc represents the size of the charge transfer impedance. If the diameter of the arc is small, it means that the charge transfer impedance of the material is small and the electrochemical activity is high. If the diameter of the arc is large, it means that the charge transfer impedance of the material is large and the electrochemical activity is low. Figure 3 The horizontal axis is the real part (Z'), the unit is ohm, and the resistance increases from left to right on the horizontal axis. Figure 3 The vertical axis is the opposite number (-Z") of the imaginary part (Z"), and the vertical axis decreases from top to bottom (-Z" from 3000 to 0), which means that the absolute value of the imaginary part is decreasing, that is, the capacitance becomes weaker and weaker as the vertical axis goes from top to bottom. Figure 3 The curve composed of pentagons represents Ti3Sn5S 12 / rGO, the circle curve represents Ti3Sn5S 12 It can be seen that Ti3Sn5S 12 The arc diameter of the / rGO curve is about 500 ohms, and the Ti3Sn5S 12The arc diameter of the curve is about 1000 ohms. 12 / rGO relative to Ti3Sn5S 12 The charge transfer impedance is smaller, the electrochemical activity is higher, and the performance is better.
[0063] The second embodiment of the present application provides a sodium ion battery negative electrode material, comprising a titanium tin sulfur compound and reduced graphene oxide, wherein the mass of the reduced graphene oxide is 15%-25% of the mass of the sodium ion battery negative electrode material. In some preferred embodiments, the mass ratio of the titanium tin sulfur compound to the reduced graphene oxide is 4:1. The sodium ion battery negative electrode material provided in the second embodiment of the present application can be prepared by any one of the methods described in the first embodiment of the present application.
[0064] The third embodiment of the present application provides a method for preparing a sodium ion battery. Figure 4 A flowchart of a method for preparing a sodium ion battery provided in the third embodiment of the present application is provided below in combination with Figure 4 The method provided in this embodiment is described in detail. Figure 4 As shown, the method for preparing a sodium ion battery provided in this embodiment includes the following steps:
[0065] S301, grinding the sodium ion battery negative electrode material, the conductive agent and the adhesive to obtain a sixth mixture, wherein the sodium ion battery negative electrode material is the sodium ion battery negative electrode material provided in the second embodiment of the present application. Specifically, the sodium ion battery negative electrode material, the conductive carbon black and the sodium carboxymethyl cellulose in a mass ratio of 80:10:10 can be ground and evenly mixed together to obtain a mixture of the ground sodium ion battery negative electrode material, the conductive carbon black and the sodium carboxymethyl cellulose. For ease of description, the mixture of the ground sodium ion battery negative electrode material, the conductive carbon black and the sodium carboxymethyl cellulose is referred to as the sixth mixture. That is, as an embodiment, the mass ratio of the sodium ion battery negative electrode material, the conductive agent and the adhesive can be 80:10:10, the conductive agent can be conductive carbon black, the adhesive can be sodium carboxymethyl cellulose, and the sodium ion negative electrode material can be made by any of the methods described in the first embodiment of the present application. The sodium ion battery negative electrode material is a key material for storing energy in the battery, and it must have high sodium ion diffusivity and reversible sodium ion insertion / extraction capabilities. The main function of the conductive agent is to improve the conductivity of the electrode material and ensure the rapid transmission of electrons inside the electrode. Conductive agents usually have high conductivity and a large specific surface area, which helps to form a good electron transmission network. Commonly used conductive agents include carbon black, graphene, carbon nanotubes, etc. The adhesive is used to bond the negative electrode material, the conductive agent and the electrode current collector (such as copper foil) together to form a stable electrode structure. The adhesive needs to have good bonding properties and electrochemical stability to ensure the structural integrity of the electrode during the charge and discharge process. Commonly used adhesives include polyvinylidene fluoride, sodium carboxymethyl cellulose and styrene-butadiene rubber.
[0066] S302, take deionized water as a solvent, mix the sixth mixture with the deionized water to obtain a slurry. Specifically, use a syringe to measure an appropriate amount of deionized water as a solvent, mix the sixth mixture with deionized water, and the mixture formed by mixing the sixth mixture with deionized water is the prepared negative electrode slurry. Negative electrode slurry is a key material used in the battery manufacturing process. It is mainly composed of active substances (in this embodiment, active substances refer to sodium ion battery negative electrode materials prepared according to any one of the methods described in the first embodiment of the present application), conductive agents, binders, etc. These solid particles are dispersed in a suitable solvent to form a special fluid, namely negative electrode slurry. In the manufacturing process of the battery, this slurry is evenly coated on the current collector (usually copper foil) through a coating process, and then undergoes subsequent process steps such as drying to form the negative electrode part of the battery. The use of deionized water can avoid the negative impact of ionic impurities on battery performance. During the mixing process, deionized water helps to form a uniform slurry, which is convenient for coating and drying processes.
[0067] S303, stirring the slurry, and applying the stirred slurry on the copper foil. Specifically, the stirring time of the slurry is 8 hours to 10 hours, and the stirred slurry is applied on the copper foil. That is, in one embodiment, the stirring time of the slurry is 8 hours to 10 hours.
[0068] S304, after the surface of the copper foil coated with the stirred slurry is air-dried, the copper foil after the surface is air-dried is dried to obtain the copper foil after the drying process as the negative electrode sheet of the sodium ion battery; specifically, after the surface of the copper foil coated with the stirred slurry is air-dried, the copper foil after the surface is air-dried is placed in a vacuum oven, and dried at a temperature of 80°C for 12 hours, and the electrode sheet is punched after the drying is completed. Among them, the drying process is to remove the solvent in the slurry and solidify the binder; punching the electrode sheet refers to punching the large piece of complete copper foil coated with the negative electrode slurry that has been dried to form an electrode sheet with a certain size to meet the structural requirements of the battery. For example, the large piece of complete copper foil can be punched into multiple circular electrode sheets with a diameter of 14 mm to make the negative electrode of the button battery. That is, as an embodiment, the drying process of the copper foil after the surface is air-dried includes: placing the copper foil after the surface is air-dried in a vacuum oven, and drying it at a temperature of 80°C for 12 hours.
[0069] S305, using glass fiber as a diaphragm material of the sodium ion battery, and using a sodium sheet as a counter electrode and a reference electrode of the sodium ion battery;
[0070] S306, a sodium ion battery is obtained according to the negative electrode sheet, the diaphragm material, the counter electrode and the reference electrode. Specifically, a sodium ion battery can be obtained in a glove box with argon gas according to the negative electrode sheet, the diaphragm material, the counter electrode and the reference electrode. The glove box filled with Ar (argon gas) provides an anhydrous and oxygen-free environment to prevent the battery materials from reacting with moisture and oxygen in the air, thereby ensuring battery performance and safety. Glass fiber is used as a diaphragm, which allows ions to pass directly while preventing the electrode materials from direct contact and short circuit. The sodium sheet can be used as a counter electrode and a reference electrode.
[0071] The sodium ion battery can be prepared by the above steps. The sodium ion battery adopts the sodium ion battery negative electrode material prepared by the sodium ion negative electrode material preparation method of the first embodiment of the present application, and thus comprises Ti3Sn5S 12 / rGO, Ti3Sn5S 12 / rGO is compounded with rGO, the density of rGO is very low, and the gap structure is very stable and tight, so it can prevent the deformation of the lattice and the expansion of the material, and can improve the stability of the negative electrode material of the sodium ion battery. 12Titanium, an inert element of sodium, is also introduced into / rGO, which not only improves the conductivity, but also alleviates the volume expansion of the negative electrode material of the sodium-ion battery to a certain extent, and improves the stability of the sodium-ion battery during the charging and discharging process.
[0072] In some embodiments, those skilled in the art may also adopt other sodium ion battery preparation methods. Specifically, the sodium ion battery negative electrode material adopted is the sodium ion battery negative electrode material provided in the second embodiment of the present application.
[0073] The fourth embodiment of the present application provides a sodium ion battery negative electrode material Ti3Sn5S 12 The preparation method of / rGO comprises the following steps: 0.189g TiCl4, 0.376g SnCl2·2H2O and 0.304g thiourea are sequentially added into a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml anhydrous ethanol is added to obtain a mixture, and the obtained mixture is stirred for 10 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h. Weigh 0.1g Ti3Sn5S 12 The mixture was mixed with 0.025 g rGO and ground evenly, and then put into a planetary ball mill and milled at a speed of 400 r / min for 8 h to obtain Ti3Sn5S 12 / rGO.
[0074] The fifth embodiment of the present application provides a sodium ion battery negative electrode material Ti3Sn5S 12 The preparation method of / rGO comprises the following steps: 0.189g TiCl4, 0.376g SnCl2·2H2O and 0.304g thiourea are added into a 50mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45ml anhydrous ethanol is added, and the resulting mixture is stirred for another 5 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h. Weigh 0.1g Ti3Sn5S 12 The mixture was mixed with 0.025 g rGO and ground evenly, and then put into a planetary ball mill and milled at a speed of 400 r / min for 8 h to obtain Ti3Sn5S 12 / rGO.
[0075] The sixth embodiment of the present application provides a sodium ion battery negative electrode material Ti3Sn5S 12The preparation method of / rGO comprises the following steps: 0.189g TiCl4, 0.376g SnCl2·2H2O and 0.304g thiourea are sequentially added into a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml anhydrous ethanol is added, and the resulting mixture is stirred for another 5 minutes. The autoclave is sealed and kept at 180°C for 13 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h. Weigh 0.1g Ti3Sn5S 12 The mixture was mixed with 0.025 g rGO and ground evenly, and then put into a planetary ball mill and milled at a speed of 400 r / min for 8 h to obtain Ti3Sn5S 12 / rGO.
[0076] The seventh embodiment of the present application provides a sodium ion battery negative electrode material Ti3Sn5S 12 The preparation method of / rGO comprises the following steps: 0.189g TiCl4, 0.376g SnCl2·2H2O and 0.304g thiourea are added into a 50mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45ml anhydrous ethanol is added, and the resulting mixture is stirred for another 5 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 50°C for 5h. Weigh 0.1g Ti3Sn5S 12 The mixture was mixed with 0.025 g rGO and ground evenly, and then put into a planetary ball mill and milled at a speed of 400 r / min for 8 h to obtain Ti3Sn5S 12 / rGO.
[0077] The eighth embodiment of the present application provides a sodium ion battery negative electrode material Ti3Sn5S 12 The preparation method of / rGO comprises the following steps: 0.189g TiCl4, 0.376g SnCl2·2H2O and 0.304g thiourea are added into a 50mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45ml anhydrous ethanol is added, and the resulting mixture is stirred for another 5 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h. Weigh 0.09g Ti3Sn5S 12 The mixture was mixed with 0.001 g rGO and ground evenly, and then put into a planetary ball mill and milled at a speed of 400 r / min for 8 h to obtain Ti3Sn5S 12 / rGO.
[0078] The ninth embodiment of the present application provides a sodium ion battery negative electrode material Ti3Sn5S 12The preparation method of / rGO comprises the following steps: 0.189g TiCl4, 0.376g SnCl2·2H2O and 0.304g thiourea are added into a 50mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45ml anhydrous ethanol is added, and the resulting mixture is stirred for another 5 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h. Weigh 0.1g Ti3Sn5S 12 The mixture was mixed with 0.025 g rGO and ground evenly, and then put into a planetary ball mill and milled at a speed of 300 r / min for 9 h to obtain Ti3Sn5S 12 / rGO.
[0079] In order to reflect the Ti3Sn5S 12 / rGO performance, this application also provides the following three comparative examples.
[0080] Comparative Example 1: 0.189 g TiCl4, 0.376 g SnCl2·2H2O and 0.304 g thiourea were added to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45 ml of anhydrous ethanol was added, and the resulting mixture was stirred for another 10 minutes. The autoclave was sealed and kept at 200°C for 12 hours. After the reaction was completed, the black fluffy product was filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4 hours. Weigh 0.1 g Ti3Sn5S 12 Grind evenly, put it into a planetary ball mill and mill it at a speed of 400r / min for 8h to obtain Ti3Sn5S 12 ;
[0081] Comparative Example 2: 0.189g TiCl4 and 0.152g thiourea were added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45ml anhydrous ethanol was added, and the resulting mixture was stirred for another 10 minutes. The autoclave was sealed and kept at 200°C for 12 hours. After the reaction was completed, the black fluffy product was filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h. Weigh 0.1g TiS2 and grind it evenly, put it into a planetary ball mill and mill it at a speed of 400r / min for 8h to obtain TiS2 / rGO;
[0082] Comparative Example 3: 0.226g SnCl2·2H2O and 0.076g thiourea were added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45ml anhydrous ethanol was added, and the resulting mixture was stirred for another 10 minutes. The autoclave was sealed and kept at 200°C for 12 hours. After the reaction was completed, the black fluffy product was filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain SnS. Weigh 0.1g SnS and 0.025g rGO, mix and grind evenly, put into a planetary ball mill and mill at a speed of 400r / min for 8h to obtain SnS / rGO;
[0083] Compared with the Ti3Sn5S prepared in the fourth to ninth embodiments of the present application 12 Compared with rGO, Comparative Example 1 is Ti3Sn5S without rGO composite. 12 Comparative Example 2 is a preparation method of TiS2 / rGO without adding tin element, and Comparative Example 3 is a preparation method of SnS / rGO without adding titanium element.
[0084] The following Table 1 shows the comparison between the fourth to ninth embodiments of the present application and comparative examples 1 to 3 in terms of initial discharge capacity, capacity retention rate, and charge transfer impedance.
[0085] Table 1 Comparison of the fourth to ninth embodiments and comparative examples 1 to 3 in terms of initial discharge capacity, capacity retention rate, and charge transfer impedance
[0086]
[0087] Among them, the initial discharge capacity refers to the amount of charge that the battery can release during the first discharge process. It reflects the ability of the battery to store energy when it is used for the first time. The higher the initial discharge capacity, the better the battery performance.
[0088] Capacity retention is a measure of how well a battery retains its ability to store energy after a certain number of charge and discharge cycles. The capacity retention after 50 cycles (compared to the second discharge capacity) is the ratio of the battery's current discharge capacity to its discharge capacity at the second discharge after 50 charge and discharge cycles. Batteries may experience performance degradation during cycling due to electrochemical reactions, changes in material structure, electrolyte decomposition, loss of active substances, etc., which results in a decrease in their ability to store energy. This indicator is used to evaluate the cycle stability and long-term reliability of batteries or electrochemical capacitors. A high capacity retention means that the device can maintain a high energy output capacity even after many cycles.
[0089] Charge transfer impedance refers to the resistance encountered when charge is transferred between the electrode and electrolyte interface during the electrochemical process. A smaller charge transfer impedance indicates that the electrochemical reaction proceeds smoothly on the electrode surface and the reaction is reversible.
[0090] As can be seen from Table 1, compared with the fourth to ninth embodiments of the present application, the initial discharge capacity, capacity retention rate and charge transfer impedance of Comparative Examples 1 to 3 are not stable, the capacity retention rate is lower, and the charge transfer impedance is higher. This further illustrates that the Ti3Sn5S prepared in the embodiments of the present application 12 The performance of / rGO is stable and good, and rGO, tin (Sn) and titanium (Ti) are all indispensable.
[0091] After research, the applicant found that in addition to Ti3Sn5S 12 In addition, Cu3SnS4 (CTS, C stands for copper, T stands for tin, and S stands for sulfur) is also a typical ternary tin-based compound with multiple advantages. First, it has a high theoretical specific capacity (719.6 mAh g -1 ). The theoretical specific capacity of Cu3SnS4 is 719.6mAh / g, which is a relatively high value, indicating that Cu3SnS4 has a large sodium storage capacity. Secondly, during the operation of the battery, the introduction of sodium-inactive element copper with high electronic conductivity can effectively improve the conductivity of the battery material and alleviate the volume effect of the battery during the charge and discharge cycle to a certain extent, thereby improving the electrochemical performance of the battery. However, compared with the theoretical specific capacity, the exposed CTS particles show insufficient reversible capacity and fast capacity decay in practical applications. Regarding the defects of CTS particles in practical applications, the applicant has found through research that reduced graphene oxide (rGO, Reduced Graphene Oxider) has excellent conductivity and mechanical properties, and is a negative electrode additive that helps to alleviate volume changes during charge and discharge cycles and improve electrochemical performance. Therefore, the preparation of ternary tin-based sulfides anchored on reduced graphene oxide can obtain high reversible capacity and good cycle stability.
[0092] Based on the above analysis, the tenth embodiment of the present application uses Cu3SnS4 / rGO as the negative electrode material of the sodium ion battery. When preparing the negative electrode material of the sodium ion battery, Cu3SnS4 can be first synthesized by a solvent thermal method, and then the Cu3SnS4 / rGO composite material can be prepared by a ball milling method. The composite material can buffer the volume expansion of the sodium ion battery during the charge and discharge process and promote the rapid transfer of electrons.
[0093] The tenth embodiment of the present application provides a method for preparing a negative electrode material for a sodium ion battery. Figure 5The preparation method of the negative electrode material of the sodium ion battery provided in the tenth embodiment of the present application is shown in the following figure. Figure 5 The method provided in this embodiment is described in detail. Figure 5 As shown, the method for preparing the negative electrode material of a sodium ion battery provided in this embodiment comprises the following steps:
[0094] S1001, add copper chloride dihydrate, tin dichloride dihydrate and thiourea in turn to a stainless steel autoclave lined with polytetrafluoroethylene, add anhydrous ethanol to the stainless steel autoclave to obtain a seventh mixture. Specifically, 0.511g of copper chloride dihydrate (CuCl2·2H2O), 0.226g of tin dichloride dihydrate (SnCl2·2H2O) and 0.304g of thiourea can be added in turn to a 50ml stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml of anhydrous ethanol is added to the stainless steel autoclave to obtain a mixture of copper chloride dihydrate, tin dichloride dihydrate, thiourea and anhydrous ethanol. For ease of description, the mixture obtained here is referred to as the seventh mixture. Copper chloride dihydrate (CuCl2·2H2O) is a copper source, and copper element (Cu) is released during high temperature treatment. Copper has good plasticity and can maintain structural integrity when the volume of the material changes. Therefore, the introduction of copper can alleviate the volume effect to a certain extent. Copper is a sodium inactive element, that is, copper does not react electrochemically with sodium, thereby alleviating the volume change caused by ion insertion and deinsertion during the electrochemical reaction. Tin dichloride dihydrate (SnCl2·2H2O) is used as a tin source to provide tin element (Ti) during the reaction process and is one of the key materials for the formation of ternary tin-based compounds. Tin-based negative electrode materials can store more charge. The alloying ability of tin allows it to absorb and release a large amount of sodium ions during the charge and discharge process, thereby improving the energy density of the material. Thiourea is a sulfur-containing compound that can participate in the reaction as a sulfur source and help form sulfide materials. Polytetrafluoroethylene (PTFE) is used as a lining for stainless steel autoclaves. It is suitable for use in high-temperature synthesis processes, which can ensure the smooth progress of the synthesis process and improve the quality and purity of the product. Anhydrous ethanol is used as a solvent to help form a uniform slurry, which is equivalent to providing a uniform reaction environment, which helps the reactants to fully contact and react, thereby improving the reaction efficiency.
[0095] Please refer to Figure 5 , after executing S1001, executing S1002, that is, after stirring the seventh mixture, an eighth mixture is obtained. Specifically, the seventh mixture can be stirred for 10 minutes, and stirring can make all reactants fully contact and prevent the reactants from being excessively concentrated in local areas. For ease of description, the mixture obtained after stirring is referred to as the eighth mixture. That is, as an embodiment, the duration of stirring the seventh mixture is 10 minutes.
[0096] After executing S1002, execute S1003, that is, seal the stainless steel autoclave containing the eighth mixture, and place the sealed stainless steel autoclave in a preset third high temperature environment for a third preset time. Specifically, the stainless steel autoclave containing the eighth mixture can be sealed at 200°C for 12 hours, and the reaction can be completed. That is, as an embodiment, the preset third high temperature environment can refer to an environment of 200°C, and the third preset time can refer to 12 hours.
[0097] S1004, obtaining a third product after high temperature treatment from a stainless steel autoclave placed in a third preset high temperature environment for a third preset time. Specifically, after the stainless steel autoclave containing the eighth mixture is sealed and maintained at 200° C. for 12 hours, a product after high temperature treatment can be obtained from the stainless steel autoclave. As an example, this product can be a black fluffy product filtered out from the stainless steel autoclave.
[0098] S1005, washing the third product to obtain a fourth product. Specifically, the third product can be washed several times with ethanol and distilled water to obtain the fourth product. As an embodiment, ethanol and distilled water can be used to remove the solvent and other soluble impurities remaining on the surface of the black fluffy product to obtain a washed black fluffy product, which is the fourth product.
[0099] S1006, placing the fourth product in a preset fourth suitable temperature environment for a fourth preset time, and performing a drying process to obtain a copper-tin-sulfur product. Specifically, the washed black fluffy product can be placed in a 60°C environment and vacuum dried for 4 hours to obtain a Cu3SnS4 solid, which is the copper-tin-sulfur product. That is, as an embodiment, the preset fourth high temperature environment can refer to an environment of 60°C, the fourth preset time can refer to 4 hours, and the drying process is performed in a vacuum environment.
[0100] S1007, mixing the copper-tin-sulfur product with reduced graphene oxide to obtain a ninth mixture. Specifically, the copper-tin-sulfur product with a mass ratio of 4:1 can be mixed with reduced graphene oxide. For example, 0.1 grams of Cu3SnS4 and 0.025 grams of rGO can be weighed and mixed to obtain a mixture of Cu3SnS4 and rGO. That is, as an embodiment, the copper-tin-sulfur product with a mass ratio of 4:1 can be mixed with reduced graphene oxide to obtain a mixture of the copper-tin-sulfur product and reduced graphene oxide. For ease of description, the mixture obtained here is referred to as the ninth mixture.
[0101] S1008, grinding the ninth mixture to obtain a tenth mixture. For example, the mixture of Cu3SnS4 and rGO can be ground evenly. For ease of description, the mixture of Cu3SnS4 and rGO after grinding evenly is referred to as the tenth mixture.
[0102] S1009, ball-milling the tenth mixture to obtain the eleventh mixture as the negative electrode material of the sodium ion battery. As an embodiment, the mixture of Cu3SnS4 and rGO after uniform grinding can be put into a planetary ball mill and ball-milled at a speed of 400 revolutions (r) / minute (min) for 8 hours to obtain a mixture of Cu3SnS4 and rGO after ball milling. For ease of description, the mixture of Cu3SnS4 and rGO after ball milling is referred to as the eleventh mixture. The eleventh mixture can be used as the negative electrode material of the sodium ion battery.
[0103] Since the tenth embodiment of the present application proposes to introduce rGO into the negative electrode material of the sodium ion battery. rGO has excellent electronic conductivity, can enhance the structural stability of the composite material, maintain the structural integrity of the electrode material during the charge and discharge process, and also help to alleviate the problem of material rupture or delamination caused by volume expansion. It can also reduce the breakage and shedding of electrode materials during the cycle and extend the service life of the battery. The channels present in the rGO layered structure may also contribute to the diffusion of sodium ions, improve the ion transport performance of the material, and thus increase the charge and discharge rate of the battery. In addition, rGO also has a higher specific surface area, which helps to increase the contact area between the electrode and the electrolyte, thereby increasing the reaction activity of the electrode. These factors work together to help achieve the development of high-performance sodium ion batteries.
[0104] The sodium ion battery negative electrode material prepared in the tenth embodiment of the present application can be Cu3SnS4 / rGO, and rGO is compounded in Cu3SnS4 / rGO. The density of rGO is very low, and the gap structure is very stable and tight, so it can prevent the deformation of the lattice and the expansion of the material, thereby improving the stability and performance of the material. Compared with the existing sulfide tin negative electrode materials, the sodium inert element copper is also introduced into Cu3SnS4 / rGO, which can not only improve the conductivity, but also alleviate the volume expansion to a certain extent, and improve the stability of the sodium ion battery during the charge and discharge process. In other specific embodiments, the above-mentioned composite rGO can also be replaced by carbon nanotubes, carbon nanofibers, Mxene, nitrogen-doped carbon, hollow carbon spheres, hard carbon, and soft carbon.
[0105] In addition, the theoretical specific capacity of Cu3SnS4 can also be calculated according to the following chemical reaction equation:
[0106]
[0107] According to the alloying reaction and conversion reaction mechanism in the above chemical reaction equation, 4 mol of Cu3SnS4 reacts with sodium (Na) ions to transfer 47 mol of electrons, that is, 1 mol of Cu3SnS4 reacts with sodium (Na) ions to transfer 11.75 mol of electrons. According to the theoretical capacity calculation formula: 96485*n / (M*3.6), 96485 is the Faraday constant, n is the number of moles of electrons transferred during the electrochemical reaction, which is 11.75 in this equation, and M is the relative molecular mass of the compound, which refers to the relative molecular mass of Cu3SnS4 in this equation. The relative molecular mass of Cu3SnS4 is 437.568. Therefore, the theoretical specific capacity of Cu3SnS4 can be calculated to be 719.6 mAh g -1 Among them, the alloying reaction mechanism here refers to the alloying reaction between tin and sodium ions to provide capacity, and the conversion reaction mechanism here refers to the conversion reaction between the material and sodium ions to provide capacity. Because there is electron transfer in the reaction, capacity can be provided.
[0108] Figure 6 is the XRD pattern of Cu3SnS4 / rGO provided in the tenth embodiment of the present application;
[0109] Among them, the full name of XRD pattern is X-ray diffraction pattern, which is a pattern obtained by X-ray diffraction technology and is used to analyze the crystal structure and other properties of the material. Figure 6 As shown, the horizontal axis represents the angle 2θ, specifically the diffraction angle of the X-ray after the X-ray interacts with the sample, and the unit is usually degree. Figure 6 The vertical axis in the graph represents the diffraction intensity detected at a specific diffraction angle, which reflects the scattering ability of the crystal plane to X-rays at that diffraction angle. The number and position of the diffraction peaks in the XRD graph can be used to determine the crystal structure and phase composition of the sample. By comparing with the standard peak graph, specific crystals in the sample can be identified. Figure 6 The lower middle line represents the standard peak diagram of Cu3SnS4 / rGO in the XRD diagram. Figure 6 The upper line represents the XRD pattern of the material prepared by the preparation method of the tenth embodiment of the present application. Figure 6It can be seen that the number and position of the diffraction peaks of the upper and lower lines can correspond, and Cu3SnS4 / rGO can match the standard diffraction peaks of Cu3SnS4 (No.33-0501) well. Based on the X-ray diffraction spectrum of rGO, no diffraction peaks of reduced graphene oxide between 2θ=20-30° were observed, indicating that Cu3SnS4 has actually covered the surface of the reduced graphene oxide sheet, while suppressing the tendency of the reduced graphene oxide sheet to re-deposit into graphite during the synthesis process. Therefore, it can be determined that the substance prepared by the preparation method of the tenth embodiment of the present application is Cu3SnS4 / rGO, and not other substances.
[0110] Figure 7 The 0.2A g of Cu3SnS4 / rGO and Cu3SnS4 provided in the tenth embodiment of the present application -1 Cycle capacity diagram. Figure 7 The horizontal axis represents the number of cycles, and the vertical axis represents the specific capacity. Figure 7 Characterizes the change of the specific capacity of Cu3SnS4 / rGO and Cu3SnS4 with the increase of charge and discharge cycles. The lines composed of circles represent Cu3SnS4, and the lines composed of pentagons represent Cu3SnS4 / rGO. Figure 7 It can be clearly seen that the specific capacity value of Cu3SnS4 composited with rGO (i.e., Cu3SnS4 / rGO) is higher than that of single Cu3SnS4.
[0111] Figure 8 This is the electrochemical impedance spectrum of Cu3SnS4 / rGO and Cu3SnS4 provided in the tenth embodiment of the present application. Figure 8 The curve composed of pentagons represents Cu3SnS4 / rGO, and the curve composed of circles represents Cu3SnS4. It can be seen that the arc diameter of the Cu3SnS4 / rGO curve is about 500 ohms, and the arc diameter of the Cu3SnS4 curve is about 1500 ohms. Therefore, Cu3SnS4 / rGO has a smaller charge transfer impedance than Cu3SnS4, has a higher electrochemical activity, and has better performance.
[0112] The eleventh embodiment of the present application provides a sodium ion battery negative electrode material, comprising a copper tin sulfur compound and reduced graphene oxide, wherein the mass of the reduced graphene oxide is 15%-25% of the mass of the sodium ion battery negative electrode material. In some preferred embodiments, the mass ratio of the copper tin sulfur compound to the reduced graphene oxide is 4:1. The sodium ion battery negative electrode material provided in the eleventh embodiment of the present application can be prepared by any one of the methods described in the tenth embodiment of the present application.
[0113] The twelfth embodiment of the present application provides a method for preparing a sodium ion battery, such as Fig. 9As shown, the method for preparing a sodium ion battery provided in this embodiment includes the following steps:
[0114] S1201, grinding the sodium ion battery negative electrode material, the conductive agent and the adhesive to obtain the twelfth mixture, wherein the sodium ion battery negative electrode material is the sodium ion battery negative electrode material provided according to the eleventh embodiment of the present application. Specifically, the sodium ion battery negative electrode material, the conductive agent and the adhesive in a mass ratio of 80:10:10 can be ground and uniformly mixed together to obtain a mixture. For the convenience of description, the mixture is referred to as the twelfth mixture. That is, as an embodiment, the mass ratio of the sodium ion battery negative electrode material, the conductive agent and the adhesive can be 80:10:10, the conductive agent can be conductive carbon black, the adhesive can be sodium carboxymethyl cellulose, and the sodium ion negative electrode material can be made by the method described in any one of the tenth embodiments of the present application.
[0115] S1202, taking deionized water as a solvent, mixing the twelfth mixture with the deionized water to obtain a slurry. Specifically, using a syringe to measure an appropriate amount of deionized water as a solvent, mixing the twelfth mixture with the deionized water, and the mixture formed by mixing the twelfth mixture and the deionized water is the prepared negative electrode slurry.
[0116] S1203, stirring the slurry, and applying the stirred slurry on the copper foil. Specifically, the stirring time of the slurry is 8 hours to 10 hours, and the stirred slurry is applied on the copper foil. That is, in one embodiment, the stirring time can be 8 hours to 10 hours.
[0117] S1204, after the surface of the copper foil coated with the stirred slurry is air-dried, the copper foil after the surface is dried is dried to obtain the copper foil after the drying process as the negative electrode sheet of the sodium ion battery. Specifically, after the surface of the copper foil coated with the stirred slurry is air-dried, the copper foil after the surface is dried is placed in a vacuum oven and dried at a temperature of 80° C. for 12 hours, and the cathode sheet is punched after the drying is completed.
[0118] S1205, using glass fiber as a diaphragm material of the sodium ion battery, and using a sodium sheet as a counter electrode and a reference electrode of the sodium ion battery;
[0119] S1206, obtaining a sodium ion battery according to the negative electrode sheet, the diaphragm material, the counter electrode and the reference electrode. Specifically, in a glove box with argon gas, obtaining a sodium ion battery according to the negative electrode sheet, the diaphragm material, the counter electrode and the reference electrode.
[0120] A sodium ion battery can be prepared through the above steps. The sodium ion battery adopts the sodium ion battery negative electrode material prepared by the sodium ion negative electrode material preparation method of the tenth embodiment of the present application, and thus includes Cu3SnS4 / rGO, in which rGO is compounded, and the density of rGO is very low, and the gap structure is very stable and tight, so it can prevent the deformation of the lattice and the expansion of the material, and can improve the stability of the negative electrode material of the sodium ion battery. Sodium inert element copper is also introduced into Cu3SnS4 / rGO, which can not only improve the conductivity, but also alleviate the volume expansion of the negative electrode material of the sodium ion battery to a certain extent, and improve the stability of the sodium ion battery during the charging and discharging process.
[0121] In some embodiments, those skilled in the art may also adopt other sodium ion battery preparation methods. Specifically, the sodium ion battery negative electrode material adopted is the sodium ion battery negative electrode material provided in the eleventh embodiment of the present application.
[0122] The thirteenth embodiment of the present application provides a method for preparing Cu3SnS4 / rGO, a negative electrode material for a sodium ion battery, comprising the following steps: 0.511gCuCl2·2H2O, 0.226gSnCl2·2H2O and 0.304gthiourea are sequentially added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml of anhydrous ethanol is added, and the resulting mixture is stirred for another 10 minutes. The autoclave is sealed and kept at 200C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain Cu3SnS4. Weigh 0.1g Cu3SnS4 and 0.025g rGO, mix and grind evenly, put into a planetary ball mill and ball mill for 8h at a speed of 400r / min to obtain Cu3SnS4 / rGO.
[0123] The fourteenth embodiment of the present application provides a method for preparing Cu3SnS4 / rGO, a negative electrode material for a sodium ion battery, comprising the following steps: 0.511g CuCl2·2H2O, 0.226g SnCl2·2H2O and 0.304g thiourea are sequentially added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml of anhydrous ethanol is added, and the resulting mixture is stirred for another 5 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain Cu3SnS4. Weigh 0.1g Cu3SnS4 and 0.025g rGO, mix and grind evenly, put into a planetary ball mill and ball mill for 8h at a speed of 400r / min to obtain Cu3SnS4 / rGO.
[0124] The fifteenth embodiment of the present application provides a method for preparing Cu3SnS4 / rGO, a negative electrode material for a sodium ion battery, comprising the following steps: 0.511g CuCl2·2H2O, 0.226g SnCl2·2H2O and 0.304g thiourea are sequentially added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml of anhydrous ethanol is added, and the resulting mixture is stirred for another 10 minutes. The autoclave is sealed and kept at 180°C for 13 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain Cu3SnS4. Weigh 0.1g Cu3SnS4 and 0.025g rGO, mix and grind evenly, put into a planetary ball mill and ball mill for 8h at a speed of 400r / min to obtain Cu3SnS4 / rGO.
[0125] The sixteenth embodiment of the present application provides a method for preparing Cu3SnS4 / rGO, a negative electrode material for a sodium ion battery, comprising the following steps: 0.511g CuCl2·2H2O, 0.226g SnCl2·2H2O and 0.304g thiourea are sequentially added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml of anhydrous ethanol is added, and the resulting mixture is stirred for another 10 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 50°C for 5h to obtain Cu3SnS4. Weigh 0.1g Cu3SnS4 and 0.025g rGO, mix and grind evenly, put into a planetary ball mill and ball mill for 8h at a speed of 400r / min to obtain Cu3SnS4 / rGO.
[0126] The seventeenth embodiment of the present application provides a method for preparing Cu3SnS4 / rGO, a negative electrode material for a sodium ion battery, comprising the following steps: 0.511g CuCl2·2H2O, 0.226g SnCl2·2H2O and 0.304g thiourea are sequentially added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml of anhydrous ethanol is added, and the resulting mixture is stirred for another 10 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain Cu3SnS4. Weigh 0.09g Cu3SnS4 and 0.01g rGO, mix and grind evenly, put into a planetary ball mill and ball mill for 8h at a speed of 400r / min to obtain Cu3SnS4 / rGO.
[0127] The eighteenth embodiment of the present application provides a method for preparing Cu3SnS4 / rGO, a negative electrode material for a sodium ion battery, comprising the following steps: 0.511g CuCl2·2H2O, 0.226g SnCl2·2H2O and 0.304g thiourea are sequentially added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml of anhydrous ethanol is added, and the resulting mixture is stirred for another 10 minutes. The autoclave is sealed and kept at 200°C for 12 hours. After the reaction is completed, the black fluffy product is filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain Cu3SnS4. Weigh 0.1g Cu3SnS4 and 0.025g rGO, mix and grind evenly, put into a planetary ball mill and ball mill at a speed of 300r / min for 9h to obtain Cu3SnS4 / rGO.
[0128] In order to demonstrate the performance of Cu3SnS4 / rGO, the present application also provides the following three comparative examples.
[0129] Comparative Example 4: 0.511g CuCl2·2H2O, 0.226g SnCl2·2H2O and 0.304g thiourea were added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene in sequence, and then 45ml anhydrous ethanol was added, and the resulting mixture was stirred for another 10 minutes. The autoclave was sealed and kept at 200°C for 12 hours. After the reaction was completed, the black fluffy product was filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain Cu3SnS4. 0.1g Cu3SnS4 was weighed and mixed and ground evenly, and then put into a planetary ball mill and ball milled at a speed of 400r / min for 8h to obtain Cu3SnS4.
[0130] Comparative Example 5: 0.170g CuCl2·2H2O and 0.076g thiourea were added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml anhydrous ethanol was added, and the resulting mixture was stirred for another 10 minutes. The autoclave was sealed and kept at 200°C for 12 hours. After the reaction was completed, the black fluffy product was filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain CuS. 0.1g CuS was weighed and mixed with 0.025g rGO and ground evenly, and then placed in a planetary ball mill and ball milled at a speed of 400r / min for 8h to obtain CuS / rGO.
[0131] Comparative Example 6: 0.226g SnCl2·2H2O and 0.076g thiourea were added to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and then 45ml anhydrous ethanol was added, and the resulting mixture was stirred for another 10 minutes. The autoclave was sealed and kept at 200°C for 12 hours. After the reaction was completed, the black fluffy product was filtered out, washed with ethanol and distilled water several times, and finally vacuum dried at 60°C for 4h to obtain SnS. 0.1g SnS was weighed and mixed with 0.025g rGO and ground evenly, and then placed in a planetary ball mill and ball milled at a speed of 400r / min for 8h to obtain SnS / rGO.
[0132] Compared with the Cu3SnS4 / rGO prepared in the thirteenth to eighteenth embodiments of the present application, Comparative Example 4 is a method for preparing Cu3SnS4 without compounding with rGO, Comparative Example 5 is a method for preparing CuS / rGO without adding tin element (Sn), and Comparative Example 6 is a method for preparing SnS / rGO without adding copper element (Cu).
[0133] The following Table 2 shows the comparison of the thirteenth to eighteenth embodiments of the present application and comparative examples 4 to 6 in terms of initial discharge capacity, capacity retention rate, and charge transfer impedance.
[0134] Table 2 Comparison of the initial discharge capacity, capacity retention rate, and charge transfer impedance of the thirteenth to eighteenth embodiments and comparative examples 4 to 6
[0135]
[0136] As can be seen from Table 2, compared with the thirteenth to eighteenth embodiments of the present application, the initial discharge capacity, capacity retention rate and charge transfer impedance of Comparative Examples 4 to Comparative Examples 6 are not stable, the capacity retention rate is lower, and the charge transfer impedance is higher. This further illustrates that the performance of the Cu3SnS4 / rGO prepared in the thirteenth to eighteenth embodiments of the present application is stable and good, and the rGO, tin element (Sn) and copper element (Cu) therein are all indispensable.
[0137] Compared with the above schemes, it can be seen that the theoretical specific capacity of titanium-based compounds will be higher, and the metallic property of titanium is stronger than that of copper, so its conductivity is stronger than that of copper. The better the conductivity, the better the rate performance. Therefore, titanium-based compounds, as the negative electrode material of the above-mentioned sodium-ion battery, have better performance than copper-tin-sulfur compounds.
[0138] Although the present application is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present application. Any technical personnel in this field may make possible changes and modifications without departing from the spirit and scope of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.
Claims
1. A method for preparing a negative electrode material for a sodium ion battery, characterized in that: The following steps are involved: Adding titanium tetrachloride, tin dichloride dihydrate and thiourea in sequence into a stainless steel autoclave lined with polytetrafluoroethylene, and adding anhydrous ethanol into the stainless steel autoclave to obtain a first mixture; After stirring the first mixture, a second mixture is obtained; Sealing the stainless steel autoclave containing the second mixture, and placing the sealed stainless steel autoclave in a preset first high temperature environment for a first preset time period; Obtaining a first product after high temperature treatment from a stainless steel autoclave placed in a preset first high temperature environment for a first preset period of time; Washing the first product to obtain a second product; placing the second product under a preset second suitable temperature environment for a second preset period of time for drying to obtain a titanium tin sulfur product; mixing the titanium tin sulfur product with reduced graphene oxide to obtain a third mixture; Grinding the third mixture to obtain a fourth mixture; The fourth mixture is ball-milled to obtain a fifth mixture, which is used as a negative electrode material for a sodium ion battery.
2. The method according to claim 1, characterized in that The mass of the titanium tetrachloride is 0.189 g, the mass of the tin dichloride dihydrate is 0.376 g, the mass of the thiourea is 0.304 g, the capacity of the stainless steel autoclave is 50 ml, and the volume of the anhydrous ethanol is 45 ml.
3. The method according to claim 1, characterized in that The mixing of the titanium tin sulfur product and reduced graphene oxide comprises: mixing the titanium tin sulfur product and reduced graphene oxide in a mass ratio of 4:
1.
4. The method according to claim 3, characterized in that The mass of the titanium tin sulfur product is 0.1 gram, and the mass of the reduced graphene oxide is 0.025 gram.
5. A sodium ion battery negative electrode material, characterized in that: It comprises titanium tin sulfur compound and reduced graphene oxide, wherein the mass of the reduced graphene oxide is 15%-25% of the mass of the negative electrode material of the sodium ion battery.
6. The sodium ion battery negative electrode material according to claim 5, characterized in that: The mass ratio of the titanium tin sulfur compound to the reduced graphene oxide is 4:
1.
7. The sodium ion battery negative electrode material according to claim 5, characterized in that The sodium ion battery negative electrode material is prepared by the method described in any one of claims 1 to 4.
8. A method for preparing a sodium ion battery, characterized in that: The following steps are involved: Grinding a sodium ion battery negative electrode material, a conductive agent and a binder to obtain a sixth mixture, wherein the sodium ion battery negative electrode material is a sodium ion battery negative electrode material prepared by the method according to any one of claims 1 to 4; Taking deionized water as a solvent, mixing the sixth mixture with the deionized water to obtain a slurry; Stirring the slurry, and applying the stirred slurry on the copper foil; After the surface of the copper foil coated with the stirred slurry is air-dried, the copper foil after the surface is air-dried is subjected to drying treatment to obtain the dried copper foil as the negative electrode sheet of the sodium ion battery; Using glass fiber as the diaphragm material of the sodium ion battery and using the sodium sheet as the counter electrode and reference electrode of the sodium ion battery; A sodium ion battery is obtained according to the negative electrode sheet, the separator material, the counter electrode and the reference electrode.
9. A sodium ion battery, characterized in that: The negative electrode material of the sodium ion battery is the negative electrode material of the sodium ion battery according to any one of claims 5 to 7.
10. A method for preparing a negative electrode material for a sodium ion battery, characterized in that: The following steps are involved: adding cupric chloride dihydrate, tin dichloride dihydrate and thiourea in sequence into a stainless steel autoclave lined with polytetrafluoroethylene, and adding anhydrous ethanol into the stainless steel autoclave to obtain a seventh mixture; After stirring the seventh mixture, an eighth mixture is obtained; Sealing the stainless steel autoclave containing the eighth mixture, and placing the sealed stainless steel autoclave in a preset third high temperature environment for a third preset time period; Obtaining a third product after high temperature treatment from a stainless steel autoclave placed in a third preset high temperature environment for a third preset period of time; washing the third product to obtain a fourth product; placing the fourth product under a preset fourth suitable temperature environment for a fourth preset time period for drying to obtain a copper-tin-sulfur product; mixing the copper-tin-sulfur product with reduced graphene oxide to obtain a ninth mixture; Grinding the ninth mixture to obtain a tenth mixture; The tenth mixture is ball-milled to obtain an eleventh mixture, which is used as a negative electrode material for a sodium ion battery.