Composite positive electrode active material, preparation method thereof, composite positive electrode and battery
By covering the surface of the manganese-based positive electrode active material with high voltage resistance, the problem of poor cycling performance of the manganese-based positive electrode active material is solved, and the high rate performance and energy density of the battery are improved.
Patent Information
- Application Number
- CN202411028845.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The manganese-based positive electrode active material is prone to react with the electrolyte at high voltage, resulting in damage to the SEI film on the negative electrode surface, deterioration of the circulation performance, and the lithium ion transmission capability of the existing coating materials is poor, affecting the rate performance of the battery.
The surface of the positive electrode active material particles is coated with halide solid electrolytes with good voltage resistance and high ionic conductivity, such as Li6-ma-nbMaNbCl6+cxXc. The coating layer is formed by ball milling to improve the lithium ion transmission efficiency and isolate the electrolyte from Contact of positive electrode.
Effectively prevent side reactions, improve the cycle performance and rate performance of the battery, improve the energy density and fast charging performance of the battery, and extend the battery life.
Smart Images

Figure BDA0004969354900000231 
Figure BDA0004969354900000241
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a battery, in particular to a composite positive electrode active material, a preparation method thereof, a composite positive electrode and a battery. Background Art
[0002] With the increasing application of secondary batteries in power tools, electric bicycles, and electric vehicles, higher requirements are placed on various performance indicators of batteries. Among them, the energy density of batteries has received special attention. The energy density of batteries is closely related to the positive electrode active material. Among the commonly used positive electrode materials, the energy density of lithium iron phosphate is relatively low, and lithium nickel manganese oxide, nickel cobalt manganese ternary positive electrode materials, lithium manganese-rich positive electrode materials, lithium manganese oxide, etc. have higher energy density, but the positive electrode active material needs to be at a high working voltage (4.3V and above) to exert a higher energy density. Under high voltage, trace water in the electrolyte will react with the electrolyte salt to generate HF, inducing the trivalent manganese ions in the positive electrode active material to undergo a disproportionation reaction to generate divalent manganese ions and tetravalent manganese ions. The divalent manganese ions are in the electrolyte and migrate to the negative electrode with the electrolyte, and a reduction reaction occurs on the negative electrode side, continuously destroying the SEI film (solid electrolyte interface film) on the surface of the negative electrode. The continuous regeneration of the SEI film consumes more lithium ions, resulting in battery capacity decay and cycle performance degradation. Summary of the invention
[0003] The present invention aims at the problems existing in the prior art and provides a composite positive electrode active material, a preparation method thereof, a composite positive electrode and a battery, which can effectively solve the technical problem of poor cycle performance of batteries prepared from manganese-based positive electrode active materials.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] In a first aspect, the present invention provides a composite positive electrode active material, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, and the first halide solid electrolyte comprises Li 6-ma-nb M a N b Cl 6+cx X c ;
[0006] Wherein, M includes Zr, In or Y; N includes Nb or Ta; X includes O or F;
[0007] m, n, and x are the valence states of elements M, N, and X, respectively;
[0008] 0<a<1.5, 0≤b<1.5, 0≤cx≤2;
[0009] The positive electrode active material includes at least one of lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium-rich manganese-based positive electrode materials.
[0010] In one embodiment, the coating layer has a thickness of 0.5-3 μm.
[0011] In one embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 19-199:1.
[0012] In one embodiment, the particle size D50 of the first halide solid electrolyte is 0.1-1 μm.
[0013] In one embodiment, the voltage U at which the composite positive electrode active material starts to continuously decompose satisfies: U≥4.4V, and the ionic conductivity λ of the composite positive electrode active material satisfies: λ≥0.25mS / cm.
[0014] In one embodiment, the first halide solid electrolyte includes Li 6-ma-nb M a N b Cl6.
[0015] In one embodiment, the first halide solid electrolyte includes Li 6-ma-nb M a Cl 6-2c O.
[0016] In one embodiment, the first halide solid electrolyte includes Li 6-ma-nb M a N b Cl 6-c F c .
[0017] In one embodiment, the composite positive electrode active material is prepared by ball milling the positive electrode active material and the first halide solid electrolyte.
[0018] In a second aspect, the present invention provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0019] 1) weighing a first halide solid electrolyte and a positive electrode active material according to a mass ratio, and mixing them to form a mixed material;
[0020] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0021] The ball milling speed is 150-350 rpm, and the ball milling time is 1-10 h.
[0022] In one embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 19-199:1.
[0023] In a third aspect, the present invention provides a composite positive electrode, comprising the composite positive electrode active material described in the above technical solution.
[0024] In one embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 80%-98%.
[0025] In a fourth aspect, the present invention further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0026] In one embodiment, the battery includes an electrolyte.
[0027] In one embodiment, the electrolyte includes an ether solvent.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The present invention can effectively isolate the manganese-based positive electrode active material from direct contact with the electrolyte by coating the halide solid electrolyte on the surface of the positive electrode active material particles, effectively prevent the side reaction between the electrolyte and the manganese-based positive electrode active material, and is beneficial to the improvement of the cycle performance of the battery. Moreover, the first halide solid electrolytes contact each other to form a good lithium ion transmission path, and there is no need to add additional solid electrolytes to the composite positive electrode to improve the lithium ion transmission efficiency, which is beneficial to the improvement of the battery energy density.
[0030] The coating layer is formed on the surface of the positive electrode active material by ball milling. On the one hand, it can effectively avoid the decomposition of the halide solid electrolyte caused by the reaction between the halide solid electrolyte and the reagent during wet coating; on the other hand, it can effectively reduce the particle size of the halide electrolyte particles, thereby reducing the thickness of the coating layer and preventing the increase in battery internal resistance caused by the excessive thickness of the coating layer.
[0031] The present invention coats the surface of the positive electrode active material with a halide solid electrolyte having good pressure resistance and high ion conductivity, thereby preparing a battery having both good cycle performance and rate performance, which is beneficial to improving the fast charging performance of the electrical device.
[0032] The voltage U≥4.4V at which the coated positive electrode active material begins to continuously decompose can effectively increase the operating voltage of the battery, which is beneficial for the positive electrode active material to exert a higher capacity at a high operating voltage. DETAILED DESCRIPTION
[0033] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.
[0034] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.
[0035] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0036] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0037] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0038] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0039] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0040] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0041] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0042] During the use of the battery, especially in a high-voltage working environment, on the one hand, the electrolyte salt in the electrolyte reacts with the inevitable trace water in the battery to generate HF, which will induce the disproportionation of trivalent manganese ions in the manganese-based positive electrode active material to generate divalent manganese ions and tetravalent manganese ions. The divalent manganese ions will dissolve into the electrolyte, move to the negative electrode side, undergo a reduction reaction, and catalyze the SEI film on the negative electrode surface to decompose it, causing the continuous generation of a new SEI film on the negative electrode side, consuming lithium ions and causing the battery's cycle performance to deteriorate. To address this problem, the prior art usually uses a coating on the positive electrode particles to isolate the direct contact between the electrolyte and the positive electrode, such as metal oxides, oxide solid electrolytes, and polymer solid electrolytes. A feature of this type of coating is that it does not have the ability to transmit lithium ions or has poor lithium ion transmission capabilities. Although it solves the problem of battery cycle performance degradation to a certain extent, the lithium ion transmission performance deteriorates, causing the battery's rate performance to deteriorate. Oxide solid electrolytes have the problem of hardness, poor contact with the positive electrode material, and are not easy to make thin. The internal resistance of the battery will increase, and the battery performance will deteriorate. Polymer solid electrolytes are also not resistant to high pressure. Under high-pressure working environments, the coating layer is prone to decomposition, and the improvement in cycle performance is limited.
[0043] In order to solve the above problems, the present application provides a composite positive electrode active material, including a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer includes a first halide solid electrolyte, and the first halide solid electrolyte includes Li 6-ma-nb M a N b Cl 6+cx X c ;
[0044] Wherein, M includes Zr, In or Y; N includes Nb or Ta; X includes O or F;
[0045] m, n, and x are the valence states of elements M, N, and X, respectively;
[0046] 0<a<1.5, 0≤b<1.5, 0≤cx≤2;
[0047] The positive electrode active material includes at least one of lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium-rich manganese-based positive electrode materials.
[0048] Halide solid electrolyte is used for coating. Compared with other solid electrolytes, halide solid electrolyte has higher lithium ion conductivity and can replace electrolyte to conduct lithium ions, so that the rate performance of the battery is not affected. On the other hand, halide solid electrolyte has a soft texture, which is conducive to forming a good coating on the surface of the positive electrode active material particles.
[0049] The present invention can effectively isolate the manganese-based positive electrode active material from direct contact with the electrolyte by coating the halide solid electrolyte on the surface of the positive electrode active material particles, effectively prevent the side reaction between the electrolyte and the manganese-based positive electrode active material, and is beneficial to the improvement of the cycle performance of the battery. Moreover, the first halide solid electrolytes contact each other to form a good lithium ion transmission path, and there is no need to add additional solid electrolytes to the composite positive electrode to improve the lithium ion transmission efficiency, which is beneficial to the improvement of the battery energy density.
[0050] The first halide solid electrolyte in the present application includes Li 6-ma-nb M a N b Cl 6+cx X c , wherein M includes Zr, In or Y; N includes Nb or Ta; X includes O or F;
[0051] Substitution of Nb and Ta elements for the basic elements Zr, In or Y can help further improve the voltage resistance of the halide solid electrolyte. Similarly, substitution of O or F for the Cl position can further improve the voltage resistance of the halide solid electrolyte.
[0052] The first halide solid electrolyte of the present application may contain both the N element and the X element, or may contain only one of the N element and the X element.
[0053] In some embodiments, the first halide solid electrolyte includes Li 6-ma-nb M a N b Cl6.
[0054] In one embodiment, the first halide solid electrolyte includes Li 6-ma-nb M a Cl 6-2c O.
[0055] In one embodiment, the first halide solid electrolyte includes Li 6-ma-nbM a Cl 6-c F.
[0056] In one embodiment, the thickness of the coating layer is 0.5-3μm, specifically 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, preferably 0.5-1.5μm. If the coating layer is too thin, it is not conducive to isolating the direct contact between the electrolyte and the positive electrode active material. If the coating layer is too thick, it is not conducive to improving the energy density of the battery.
[0057] In one embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 19-199:1, specifically 19:1, 24:1, 32:1, 49:1, 65:1, 99:1, 199:1.
[0058] In one embodiment, the particle size D50 of the first halide solid electrolyte is 0.1-1 μm. By controlling the particle size of the halide solid electrolyte, it is beneficial to form a thin and uniform coating layer on the surface of the positive electrode active material particles.
[0059] In one embodiment, the voltage U at which the composite positive electrode active material starts to continuously decompose satisfies: U≥4.4V, and the ionic conductivity λ of the composite positive electrode active material satisfies: λ≥0.25mS / cm.
[0060] The present invention coats the surface of the positive electrode active material with a halide solid electrolyte having good pressure resistance and high ion conductivity, thereby preparing a battery having both good cycle performance and rate performance, which is beneficial to improving the fast charging performance of the electrical device.
[0061] The voltage U≥4.4V at which the coated positive electrode active material begins to continuously decompose can effectively increase the operating voltage of the battery, which is beneficial for the positive electrode active material to exert a higher capacity at a high operating voltage.
[0062] The voltage at which the composite positive electrode active material begins to continuously decompose can be determined by scanning the cyclic voltammetry curve using an electrochemical workstation.
[0063] In a second aspect, the present invention provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0064] 1) weighing a first halide solid electrolyte and a positive electrode active material according to a mass ratio, and mixing them to form a mixed material;
[0065] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0066] The ball milling speed is 150-350 rpm, and the ball milling time is 1-10 h.
[0067] The coating layer is formed on the surface of the positive electrode active material by ball milling. On the one hand, it can effectively avoid the decomposition of the halide solid electrolyte caused by the reaction between the halide solid electrolyte and the reagent during wet coating; on the other hand, it can effectively reduce the particle size of the halide electrolyte particles, thereby reducing the thickness of the coating layer and preventing the increase in battery internal resistance caused by the excessive thickness of the coating layer.
[0068] In one embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 19-199:1.
[0069] In one embodiment, the ball milling process is performed in an environment where the water oxygen content is less than 5 ppm. For example, the ball milling process is performed in a glove box.
[0070] In one embodiment, during the ball milling process, the mass ratio of ball milling beads to mixed materials is 1:(15-60).
[0071] In a third aspect, the present invention provides a composite positive electrode, comprising the composite positive electrode active material described in the above technical solution or the composite positive electrode active material prepared by the preparation method in the above technical solution.
[0072] In one embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 80%-98%, which can be 80%, 82%, 85%, 87%, 89%, 90%, 92%, 94%, 95%, 96%, 97%, or 98%.
[0073] In one embodiment, the composite positive electrode further includes a conductive agent, which plays a role in collecting microcurrents between active materials and between active materials and current collectors.
[0074] In one embodiment, in the composite positive electrode, the mass proportion of the conductive agent is 1-10%.
[0075] In one embodiment, the conductive agent includes graphite, such as natural graphite or artificial graphite; carbon materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; conductive fibers, such as carbon fibers and metal fibers; conductive tubes, such as carbon nanotubes; metal powders, such as fluorocarbon powders, aluminum powders and nickel powders; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; and polyphenylene derivatives, and from the aspect of improving conductivity, the positive electrode conductive agent may preferably be carbon black.
[0076] In one embodiment, the specific surface area of the conductive agent may be 80-200 m 2 / g, preferably 100-150m2 / g.
[0077] In one embodiment, the composite positive electrode further includes a binder, which can firmly adhere the composite positive electrode active material and the conductive agent in the electrode sheet together.
[0078] In one embodiment, in the composite positive electrode, the binder accounts for 1-10% by mass.
[0079] In one embodiment, the binder comprises a fiberized binder. It is understood that the fiberized binder can be transformed from a granular state to a fibrous state under the action of high shear force.
[0080] Exemplarily, the fiberized binder includes one or more of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene (PE), and polypropylene (PP).
[0081] In a preferred embodiment, the binder further includes other binders, which can be illustratively polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, styrene-butadiene rubber and fluororubber, preferably polyvinylidene fluoride. The role of other binders is to be used in conjunction with the fibrous binder to further enhance the bonding strength between the composite positive electrode active material and the conductive agent.
[0082] In one embodiment, the thickness of the composite positive active electrode material layer may be 30 μm to 400 μm, for example, 30 μm, 40 μm, 50 μm, 80 μm, 110 μm, 200 μm, 300 μm, 400 μm, preferably 50 μm to 110 μm.
[0083] In one embodiment, the positive electrode sheet can be prepared by a dry film-making method, by mixing the composite positive electrode material, conductive agent, binder and other additives, and placing them in a device that can provide high shear force, such as a mixer, a mixer, etc. Under high shear force, the binder is fiberized, and the composite positive electrode material, conductive agent and other binders are bonded together to form a composite positive electrode film by pressing. Of course, the composite positive electrode material, conductive agent, and other additives can also be mixed first, and then mixed with the binder. It is also possible to choose whether to add other additives according to actual needs.
[0084] In a fourth aspect, the present invention further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0085] In one embodiment, the battery includes an electrolyte, the electrolyte includes a solvent, and the solvent includes at least one of an ether solvent, propylene carbonate, and fluoroethylene carbonate.
[0086] In one embodiment, the battery includes an electrolyte including an ether solvent.
[0087] In one embodiment, in the electrolyte, the mass proportion of the ether solvent is 5-65%.
[0088] In one embodiment, the electrolyte further includes an electrolyte salt. Exemplarily, it can be at least one of lithium hexafluorophosphate (LiPF6), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium bisfluorosulfonyl imide (LiFSI), lithium tetrafluoroborate (LiBF4) and bistrifluoromethanesulfonyl imide (LiTFSI), lithium difluorophosphate (LiPO2F2), lithium bisoxalate borate (LiBOB), lithium bisfluorooxalate borate (LiODFB), lithium difluorobisoxalate phosphate (LiODFP) or lithium tetrafluorooxalate phosphate (LiTFOP).
[0089] In one embodiment, based on the total mass of the electrolyte being 100%, the mass percentage of the electrolyte salt is 0.5-25%.
[0090] In one embodiment, the electrolyte contains additives, and the electrolyte also includes additives, and the additives include at least one of 1,3-propane sultone, 1,4-butane sultone, propenyl-1,3-sultone, vinyl sulfate, 4-methyl vinyl sulfate, propenyl sulfate, saturated phosphate compounds and unsaturated phosphate compounds, tris(trimethylsilane) phosphate, tris(trimethylsilane) borate, tris(triethylsilane) borate, succinonitrile, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexane trinitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid nitrile, and sebaconitrile.
[0091] In one embodiment, the battery further includes a negative electrode.
[0092] In one embodiment, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer formed on the surface of the negative electrode current collector, wherein the negative electrode active material layer comprises at least a negative electrode active material and a negative electrode binder.
[0093] In one embodiment, the negative electrode active material in the embodiment of the present application is not particularly limited, as long as it is a material that can electrochemically absorb and release S-zone metal ions such as lithium ions, sodium ions, potassium ions, and magnesium ions, such as carbonaceous materials, metal compound materials, or their oxides, carbides, nitrides, silicides, sulfides, phosphides, etc. These materials can be used alone, or two or more can be used in combination.
[0094] In one embodiment, a carbon material can be selected as the negative electrode active material, and specifically one or more of the following can be selected: graphite, needle coke, amorphous carbon, a carbon-containing mesophase, carbon fiber, and a carbon material with a low degree of graphitization. Among them, graphite can include natural graphite, artificial graphite, etc. In addition, materials obtained by coating them with carbon materials, such as amorphous carbon and graphitized materials, can also be used. Amorphous carbon includes but is not limited to particles obtained by firing the entire mesophase, and particles obtained by infusible treatment and firing of a carbon precursor. As carbonaceous particles with a low degree of graphitization, particles obtained by firing organic matter at a temperature generally below 2500°C can be listed.
[0095] In one embodiment, non-metallic materials that can be used as negative electrode active materials also include silicon and its compounds, such as Si, SiOx (0≤x<2). Since silicon-containing materials are prone to expansion, easy to fall off from the negative electrode current collector, and have poor conductivity, they are often mixed with carbon materials, such as a core-shell structure containing a carbon coating layer.
[0096] In one embodiment, metal elements and metal compounds can also be selected as negative electrode active materials, such as compounds containing metals or metalloids such as Li, Ag, Al, Bi, Cu, Ga, Ge, In, Ni, Pb, Sb, Si, Sn, Sr, and Zn.
[0097] In one embodiment, the mass percentage of the negative electrode active material contained in the negative electrode active material layer may be 80-99%, for example, 80%, 85%, 90%, 95%, 97%, 99%, etc., preferably 95-97%.
[0098] In one embodiment, when the negative electrode active material is a non-metallic material such as a carbon material, the negative electrode binder may be an aqueous binder such as one or more of sodium hydroxymethyl cellulose, styrene-butadiene latex, polyacrylic acid, acrylic copolymer, cyclodextrin, etc.;
[0099] In one embodiment, the negative electrode active material layer can be obtained by coating a negative electrode slurry on a negative electrode current collector and then drying the negative electrode slurry, wherein the negative electrode slurry includes at least a negative electrode active material and a negative electrode binder. When an aqueous solvent is used as a liquid medium for forming the negative electrode slurry, a thickener is preferably used for slurrying, and the thickener can generally be used to adjust the viscosity of the slurry.
[0100] In one embodiment, the thickener in the embodiment of the present application can be one or more of the following: carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein and their salts, etc.
[0101] In one embodiment, the mass proportion of the thickener in the negative electrode slurry can be 0.1-5%, for example, 0.1%, 0.2%, 0.5%, 0.6%, 1%, 2%, 3%, 4%, 5%, etc., preferably 0.5-3%, and more preferably 0.6-2%.
[0102] The technical solution of the present invention will be further explained below in conjunction with specific embodiments. In a specific embodiment, the sum of the mass ratios of the positive electrode active material and the first halide solid electrolyte is 100%, the sum of the mass ratios of graphite, binder CMC, and conductive agent Super-p in the negative electrode is 100%, and the mass ratio of the ether solvent in the electrolyte is 15%.
[0103] Example 1
[0104] In a first aspect, the present embodiment provides a composite positive electrode active material, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, and the first halide solid electrolyte is Li 1.5 Z r0.5 Nb 0.5 Cl6, the positive electrode active material includes lithium manganate.
[0105] In this embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 99:1.
[0106] In this embodiment, the thickness of the coating layer is 0.8 μm;
[0107] In this embodiment, the particle size D50 of the first halide solid electrolyte is 0.5 μm.
[0108] In a second aspect, this embodiment provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0109] 1) weighing a first halide solid electrolyte and a positive electrode active material in a mass ratio of 1:99, and mixing them to form a mixed material;
[0110] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0111] The ball milling speed was 300 rpm, the ball milling time was 6 h, and the mass ratio of ball milling beads to mixed materials was 1:30.
[0112] In a third aspect, this embodiment provides a composite positive electrode, comprising the composite positive electrode active material.
[0113] In this embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 95%;
[0114] In this embodiment, the composite positive electrode also includes a conductive agent and a binder. Specifically, the mass ratio of the composite positive electrode active material, the conductive agent, and the binder in the composite positive electrode is 95:3:2; the conductive agent is superconducting carbon black, and the binder is polytetrafluoroethylene (PTFE).
[0115] In a fourth aspect, this embodiment further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0116] The battery also includes an electrolyte, which is composed of a solvent and an electrolyte salt. The solvent includes an ether solvent, propylene carbonate, and fluoroethylene carbonate. The electrolyte salt includes lithium hexafluorophosphate LiPF6 and lithium difluorophosphate LiPO2F2.
[0117] Specifically, in this embodiment, the mass ratio of the ether solvent (isoamyl ether), propylene carbonate, fluoroethylene carbonate, lithium hexafluorophosphate LiPF6, and lithium difluorophosphate LiPO2F2 is 15:60:10:14:1.
[0118] The battery also includes a negative electrode, and the negative electrode active material includes graphite. In the negative electrode, graphite: binder CMC: conductive agent Super-p=95:3:2.
[0119] Example 2
[0120] In a first aspect, the present embodiment provides a composite positive electrode active material, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, and the first halide solid electrolyte is Li 1.5 Z r0.5 Nb 0.5 Cl6, the positive electrode active material includes lithium manganate.
[0121] In this embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 19:1.
[0122] In this embodiment, the thickness of the coating layer is 3 μm;
[0123] In this embodiment, the particle size D50 of the first halide solid electrolyte is 1 μm.
[0124] In a second aspect, this embodiment provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0125] 1) weighing a first halide solid electrolyte and a positive electrode active material in a mass ratio of 1:19, and mixing them to form a mixed material;
[0126] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0127] The ball milling speed was 300 rpm, the ball milling time was 6 h, and the mass ratio of ball milling beads to mixed materials was 1:30.
[0128] In a third aspect, this embodiment provides a composite positive electrode, comprising the composite positive electrode active material.
[0129] In this embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 95%;
[0130] In this embodiment, the composite positive electrode also includes a conductive agent and a binder. Specifically, the mass ratio of the composite positive electrode active material, the conductive agent, and the binder in the composite positive electrode is 95:3:2; the conductive agent is superconducting carbon black, and the binder is polytetrafluoroethylene (PTFE).
[0131] In a fourth aspect, this embodiment further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0132] The battery also includes an electrolyte, which is composed of a solvent and an electrolyte salt. The solvent includes an ether solvent, propylene carbonate, and fluoroethylene carbonate. The electrolyte salt includes lithium hexafluorophosphate LiPF6 and lithium difluorophosphate LiPO2F2.
[0133] Specifically, in this embodiment, the mass ratio of the ether solvent (isoamyl ether), propylene carbonate, fluoroethylene carbonate, lithium hexafluorophosphate LiPF6, and lithium difluorophosphate LiPO2F2 is 15:60:10:14:1.
[0134] The battery also includes a negative electrode, and the negative electrode active material includes graphite. In the negative electrode, graphite: binder CMC: conductive agent Super-p=95:3:2.
[0135] Example 3
[0136] In a first aspect, the present embodiment provides a composite positive electrode active material for a battery, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, and the first halide solid electrolyte is Li 1.5 Z r0.5 Nb 0.5 Cl6, the positive electrode active material includes lithium manganate.
[0137] In this embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 199:1.
[0138] In this embodiment, the thickness of the coating layer is 0.5 μm;
[0139] In this embodiment, the particle size D50 of the first halide solid electrolyte is 0.5 μm.
[0140] In a second aspect, this embodiment provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0141] 1) weighing a first halide solid electrolyte and a positive electrode active material in a mass ratio of 1:199, and mixing them to form a mixed material;
[0142] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0143] The ball milling speed was 300 rpm, the ball milling time was 6 h, and the mass ratio of ball milling beads to mixed materials was 1:30.
[0144] In a third aspect, this embodiment provides a composite positive electrode, comprising the composite positive electrode active material.
[0145] In this embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 95%;
[0146] In this embodiment, the composite positive electrode also includes a conductive agent and a binder. Specifically, the mass ratio of the composite positive electrode active material, the conductive agent, and the binder in the composite positive electrode is 95:3:2; the conductive agent is superconducting carbon black, and the binder is polytetrafluoroethylene (PTFE).
[0147] In a fourth aspect, this embodiment further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0148] The battery also includes an electrolyte, which is composed of a solvent and an electrolyte salt. The solvent includes an ether solvent, propylene carbonate, and fluoroethylene carbonate. The electrolyte salt includes lithium hexafluorophosphate LiPF6 and lithium difluorophosphate LiPO2F2.
[0149] Specifically, in this embodiment, the mass ratio of the ether solvent (isoamyl ether), propylene carbonate, fluoroethylene carbonate, lithium hexafluorophosphate LiPF6, and lithium difluorophosphate LiPO2F2 is 15:60:10:14:1.
[0150] The battery also includes a negative electrode, and the negative electrode active material includes graphite. In the negative electrode, graphite: binder CMC: conductive agent Super-p=95:3:2.
[0151] Example 4
[0152] In a first aspect, the present embodiment provides a composite positive electrode active material for a battery, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, the first halide solid electrolyte is Li2ZrCl4O, and the positive electrode active material comprises lithium nickel manganese oxide.
[0153] In this embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 99:1.
[0154] In this embodiment, the thickness of the coating layer is 0.8 μm;
[0155] In this embodiment, the particle size D50 of the first halide solid electrolyte is 0.5 μm.
[0156] In a second aspect, this embodiment provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0157] 1) weighing a first halide solid electrolyte and a positive electrode active material in a mass ratio of 1:99, and mixing them to form a mixed material;
[0158] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0159] The ball milling speed was 300 rpm, the ball milling time was 6 h, and the mass ratio of ball milling beads to mixed materials was 1:30.
[0160] In a third aspect, this embodiment provides a composite positive electrode, comprising the composite positive electrode active material.
[0161] In this embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 95%;
[0162] In this embodiment, the composite positive electrode also includes a conductive agent and a binder. Specifically, the mass ratio of the composite positive electrode active material, the conductive agent, and the binder in the composite positive electrode is 95:3:2; the conductive agent is superconducting carbon black, and the binder is polytetrafluoroethylene (PTFE).
[0163] In a fourth aspect, this embodiment further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0164] The battery also includes an electrolyte, which is composed of a solvent and an electrolyte salt. The solvent includes an ether solvent, propylene carbonate, and fluoroethylene carbonate. The electrolyte salt includes lithium hexafluorophosphate LiPF6 and lithium difluorophosphate LiPO2F2.
[0165] Specifically, in this embodiment, the mass ratio of the ether solvent (isoamyl ether), propylene carbonate, fluoroethylene carbonate, lithium hexafluorophosphate LiPF6, and lithium difluorophosphate LiPO2F2 is 15:60:10:14:1.
[0166] The battery also includes a negative electrode, and the negative electrode active material includes graphite. In the negative electrode, graphite: binder CMC: conductive agent Super-p=95:3:2.
[0167] Example 5
[0168] In a first aspect, this embodiment provides a composite positive electrode active material for a battery, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, the first halide solid electrolyte is Li3InCl3F3, and the positive electrode active material comprises lithium manganate.
[0169] In this embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 99:1.
[0170] In this embodiment, the thickness of the coating layer is 0.8 μm;
[0171] In this embodiment, the particle size D50 of the first halide solid electrolyte is 0.5 μm.
[0172] In a second aspect, this embodiment provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0173] 1) weighing a first halide solid electrolyte and a positive electrode active material in a mass ratio of 1:99, and mixing them to form a mixed material;
[0174] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0175] The ball milling speed was 300 rpm, the ball milling time was 6 h, and the mass ratio of ball milling beads to mixed materials was 1:30.
[0176] In a third aspect, this embodiment provides a composite positive electrode, comprising the composite positive electrode active material.
[0177] In this embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 95%;
[0178] In this embodiment, the composite positive electrode also includes a conductive agent and a binder. Specifically, the mass ratio of the composite positive electrode active material, the conductive agent, and the binder in the composite positive electrode is 95:3:2; the conductive agent is superconducting carbon black, and the binder is polytetrafluoroethylene (PTFE).
[0179] In a fourth aspect, this embodiment further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0180] The battery also includes an electrolyte, which is composed of a solvent and an electrolyte salt. The solvent includes an ether solvent, propylene carbonate, and fluoroethylene carbonate. The electrolyte salt includes lithium hexafluorophosphate LiPF6 and lithium difluorophosphate LiPO2F2.
[0181] Specifically, in this embodiment, the mass ratio of the ether solvent (isoamyl ether), propylene carbonate, fluoroethylene carbonate, lithium hexafluorophosphate LiPF6, and lithium difluorophosphate LiPO2F2 is 15:60:10:14:1.
[0182] The battery also includes a negative electrode, and the negative electrode active material includes graphite. In the negative electrode, graphite: binder CMC: conductive agent Super-p=95:3:2.
[0183] Example 6
[0184] In a first aspect, the present embodiment provides a composite positive electrode active material for a battery, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, and the first halide solid electrolyte is Li 1.5 Z r0.5 Nb 0.5 Cl 4.5 O 0.25 , the positive electrode active material includes lithium manganese oxide.
[0185] In this embodiment, the mass ratio of the positive electrode active material to the first halide solid electrolyte is 13:1.
[0186] In this embodiment, the thickness of the coating layer is 5 μm;
[0187] In this embodiment, the particle size D50 of the first halide solid electrolyte is 4 μm.
[0188] In a second aspect, this embodiment provides a method for preparing the above-mentioned composite positive electrode active material, comprising the following steps:
[0189] 1) weighing a first halide solid electrolyte and a positive electrode active material in a mass ratio of 1:99, and mixing them to form a mixed material;
[0190] 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material;
[0191] The ball milling speed was 280 rpm, the ball milling time was 10 h, and the mass ratio of ball milling beads to mixed materials was 1:30.
[0192] In a third aspect, this embodiment provides a composite positive electrode, comprising the composite positive electrode active material.
[0193] In this embodiment, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 95%;
[0194] In this embodiment, the composite positive electrode also includes a conductive agent and a binder. Specifically, the mass ratio of the composite positive electrode active material, the conductive agent, and the binder in the composite positive electrode is 95:3:2; the conductive agent is superconducting carbon black, and the binder is polytetrafluoroethylene (PTFE).
[0195] In a fourth aspect, this embodiment further provides a battery, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode as described in the third aspect.
[0196] The battery also includes an electrolyte, which is composed of a solvent and an electrolyte salt. The solvent includes an ether solvent, propylene carbonate, and fluoroethylene carbonate. The electrolyte salt includes lithium hexafluorophosphate LiPF6 and lithium difluorophosphate LiPO2F2.
[0197] Specifically, in this embodiment, the mass ratio of the ether solvent (isoamyl ether), propylene carbonate, fluoroethylene carbonate, lithium hexafluorophosphate LiPF6, and lithium difluorophosphate LiPO2F2 is 15:60:10:14:1.
[0198] The battery also includes a negative electrode, and the negative electrode active material includes graphite. In the negative electrode, graphite: binder CMC: conductive agent Super-p=95:3:2.
[0199] Comparative Example 1
[0200] The difference between Comparative Example 1 and Example 1 is that no coating layer is provided on the surface of the lithium manganese oxide.
[0201] Comparative Example 2
[0202] The difference between Comparative Example 2 and Example 1 is that the first halide solid electrolyte is LLZO (Li7La3Zr2O 12 ).
[0203] Comparative Example 3
[0204] The difference from Example 1 is that the first halide solid electrolyte is Li 2.5 Zr 0.5 Al 0.5 Cl6.
[0205] Test Method
[0206] 1) Cycle performance test
[0207] The assembled batteries of Examples 1-6 and Comparative Examples 1-3 were subjected to a cycle performance test, with a charge and discharge potential range of 3.0 V to 4.4 V. The first cycle was charged and discharged at a current of 0.1 C, and the second cycle was charged and discharged at a current of 0.33 C. The cycle was repeated for 100 cycles, and the cycle retention rate was recorded. The cycle retention rate = discharge capacity at the 100th cycle / discharge capacity at the 2nd cycle.
[0208] 2) Rate performance test
[0209] The battery was placed at 25°C for 10 min, then charged to 4.4 V at a constant current rate of 0.1C, placed for 10 min, and then discharged to 3.0 V at a constant current rate of 0.1C;
[0210] Charge at a constant current of 2C to 4.4V, leave for 10 minutes, and then discharge at a constant current of 2C to 3.0V.
[0211] And calculate the capacity retention rate, capacity retention rate = 2C discharge capacity / 0.1C rate discharge capacity * 100%.
[0212] The test results are shown in Table 1:
[0213] Table 1 Battery charge and discharge performance
[0214]
[0215]
[0216] The battery charge and discharge performance test results in Table 1 show that the composite positive electrode of Examples 1-6 of the present application has a 100-cycle capacity retention rate of 93-96%, and a 2C discharge capacity retention rate of 92-95%, which has both good cycle performance and rate performance.
[0217] Comparing Example 1 with Comparative Example 1, compared with a single positive electrode active material, coating the manganese-based positive electrode active material can effectively improve the cycle performance of the battery, and the rate performance of the battery will not be significantly affected.
[0218] Comparing Example 1 with Comparative Examples 1 and 2, the use of halide solid electrolyte for coating can make the battery including the composite positive electrode active material have both good rate performance and cycle performance.
[0219] Comparing Example 1 with Comparative Example 3, the performance of the battery prepared in Example 1 is better than that in Comparative Example 3, where the halide solid electrolyte is also used as the coating material. The possible reason is that Li 2.5 Zr 0.5 Al 0.5 The oxidation resistance of Cl6 is worse than that of Li 1.5 Z r0.5 Nb 0.5 Cl6, Li 2.5 Zr 0.5 Al 0.5 The voltage at which Cl6 starts to decompose continuously is lower than 4.35V. Under long-term high voltage working environment, Li 2.5 Zr 0.5 Al 0.5Cl6 decomposes and the coating effect becomes worse. The above is only a possible speculation on the technical solution of the present application and does not constitute a limitation on the protection scope of the present application.
[0220] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0221] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A composite positive electrode active material, characterized in that: The invention comprises a positive electrode active material and a coating layer coated on the surface of the positive electrode active material particles, wherein the coating layer comprises a first halide solid electrolyte, and the first halide solid electrolyte comprises Li 6-ma-nb M a N b Cl 6+cx X c ; Wherein, M includes Zr, In or Y; N includes Nb or Ta; X includes O or F; m, n, and x are the valence states of elements M, N, and X, respectively; 0<a<1.5, 0≤b<1.5, 0≤cx≤2; The positive electrode active material includes at least one of lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium-rich manganese-based positive electrode materials.
2. The composite positive electrode active material according to claim 1, characterized in that: The coating layer has a thickness of 0.5-3 μm.
3. The composite positive electrode active material according to claim 1, characterized in that The mass ratio of the positive electrode active material to the first halide solid electrolyte is 19-199:
1.
4. The composite positive electrode active material according to claim 1, characterized in that: The particle size D50 of the first halide solid electrolyte is 0.1-1 μm.
5. The composite positive electrode active material according to claim 1, characterized in that: The voltage U at which the composite positive electrode active material starts to continuously decompose satisfies: U≥4.4V, and the ion conductivity λ of the composite positive electrode active material satisfies: λ≥0.25mS / cm.
6. The composite positive electrode active material according to claim 1, characterized in that: The first halide solid electrolyte includes Li 6-ma-nb M a N b Cl6.
7. A method for preparing a composite positive electrode active material according to any one of claims 1 to 6, characterized in that: The steps include: 1) weighing a first halide solid electrolyte and a positive electrode active material according to a mass ratio, and mixing them to form a mixed material; 2) placing the mixed material of step 1) into a ball mill and milling the mixed material to obtain a composite positive electrode active material; The ball milling speed is 150-350 rpm, and the ball milling time is 1-10 h.
8. A composite positive electrode, characterized in that: The composite positive electrode active material comprises any one of claims 1 to 6.
9. A battery, characterized in that: It comprises the composite positive electrode active material according to any one of claims 1 to 6 or the composite positive electrode according to claim 8.
10. The battery according to claim 9, characterized in that The battery also includes an electrolyte.
Citation Information
Cited By
High-voltage-resistant thick electrode, preparation method and battery cell
CN119480926A
MXene and halide solid electrolyte composite modified lithium manganese iron phosphate material as well as preparation method and application thereof
CN120527361A
Composite lithium-rich manganese-based positive electrode material and preparation method and application thereof
CN120998963A
Solid-state battery cell, solid electrolyte and method for preparing same, battery device, and electrical device
WO2026166276A1