Modified sodium ion battery positive electrode material, preparation method thereof and sodium ion battery

The polymer conductive polymer coating of the layered oxide positive electrode material of sodium ion battery is coated with sodium ion battery through water washing coating, which solves the problem of poor material circulation performance, improves the capacity and circulation performance, and reduces production costs and achieves more Highly efficient sodium ion battery performance.

CN118943345APending Publication Date: 2024-11-12XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411344793.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Due to the large sodium ion radius of the sodium ion battery, the layered oxide positive electrode material is prone to damage to the layered structure during the de-embedding process, resulting in poor circulation performance of the material, poor air stability and strong water absorption, resulting in low capacity and circulation performance. Not good.

Method used

The layered oxide positive electrode material is coated with polymer conductive polymer by washing coating. By forming a short chain coating on the surface of the material, it hinders the contact of moisture in the air, inhibits the exchange of sodium ions and water molecules, and maintains the crystal structure. Stable and improve sodium ion transfer rate.

Benefits of technology

The capacity and circulation performance of the layered oxide positive electrode material have been significantly improved. The capacity of the modified sodium ion battery positive electrode material reaches 135.1mAh/g at room temperature. The capacity retention rate reaches 76% after 50 cycles, but it has not been modified. The material is only 68%, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005060663880000061
    Figure BDA0005060663880000061
  • Figure BDA0005060663880000111
    Figure BDA0005060663880000111
  • Figure BDA0005060663880000121
    Figure BDA0005060663880000121
Patent Text Reader

Abstract

The invention relates to the technical field of sodium ion batteries, in particular to a modified sodium ion battery positive electrode material, a preparation method thereof and a sodium ion battery, the preparation method comprises the following steps: S1, weighing an M source and a sodium source, uniformly mixing the M source and the sodium source, and calcining to obtain a mixture 1, the M source comprises at least one of a Ni source, a Fe source, a Mn source, a Cu source and a Co source; s2, adding a high-molecular conductive polymer into water in a water washing kettle, adding the mixture 1 into the water washing kettle, and stirring to obtain a mixture 2; and S3, centrifuging and drying the mixture 2 in the step S2 to obtain the modified sodium ion battery positive electrode material. According to the invention, the layered oxide positive electrode material is coated with the high-molecular conductive polymer by adopting a washing coating method, so that the gram volume and the cycle performance of the layered oxide positive electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a modified sodium ion battery positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] In recent years, the shortage of lithium resources has led to an increase in the cost of lithium-ion batteries, and sodium, which is abundant in reserves and has a lower cost, has once again come into people's view. The energy density of sodium-ion batteries is not as high as that of lithium-ion batteries, but their stable electrochemical performance and high cost-effectiveness give them outstanding advantages in energy storage, two-wheeled vehicles and other fields. The structure and principle of sodium-ion batteries are similar to those of lithium-ion batteries. The main positive electrode materials of sodium-ion batteries are layered metal oxides, Prussian blue, polyanions, etc. Among them, layered metal oxides have high energy density, relatively simple synthesis, and their structure is similar to that of lithium-ion battery positive electrode materials, and their application range is relatively wide.

[0003] Conventional sodium-ion battery layered oxide cathode materials are prone to damage to the layered structure during the deintercalation process due to the large radius of sodium ions, resulting in poor material cycle performance. In addition, sodium-ion battery layered oxide cathode materials have poor air stability and strong water absorption. After the material surface absorbs water molecules, sodium ions in the bulk phase will precipitate, causing the material crystal structure to change or even be destroyed, which will eventually cause the battery to have low gram capacity and poor cycle performance.

[0004] Therefore, how to improve the gram capacity and cycle performance of layered oxide positive electrode materials for sodium ion batteries is a technical problem that needs to be urgently solved in this technical field. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a modified sodium ion battery positive electrode material, a preparation method thereof and a sodium ion battery. The present invention improves the gram capacity and cycle performance of the layered oxide positive electrode material by coating the layered oxide positive electrode material with a high molecular conductive polymer using a water washing coating method.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a modified sodium ion battery positive electrode material, the preparation method comprising the following steps:

[0008] S1, weighing an M source and a sodium source, mixing the M source and the sodium source uniformly and then calcining to obtain a mixture 1, wherein the M source includes at least one of a Ni source, a Fe source, a Mn source, a Cu source, and a Co source;

[0009] S2, adding a high molecular conductive polymer to the water in a water washing kettle, and then adding the mixture 1 to the water washing kettle, and obtaining a mixture 2 after stirring;

[0010] S3, centrifuging and drying the mixture 2 in step S2 to obtain a modified sodium ion battery positive electrode material.

[0011] The present invention coats the layered oxide positive electrode material with a high molecular conductive polymer by adopting a water washing coating method, thereby improving the gram capacity and cycle performance of the layered oxide positive electrode material.

[0012] Furthermore, the Ni source includes at least one of nickel sulfate and nickel nitrate, the Fe source includes at least one of iron sulfate and iron nitrate, the Mn source includes at least one of manganese sulfate and manganese nitrate, the Cu source includes at least one of copper sulfate and copper nitrate, the Co source includes at least one of cobalt sulfate and cobalt nitrate, and the sodium source includes at least one of sodium carbonate, sodium chloride and sodium sulfate.

[0013] Furthermore, the high molecular conductive polymer includes at least one of PEDOT, polythiophene, and polypyrrole;

[0014] And / or, in step S2, the high molecular conductive polymer is added to the water in the water washing kettle in the form of a high molecular conductive polymer / PSS aqueous solution.

[0015] Furthermore, in step S2, the mass percentage of the high molecular conductive polymer in the high molecular conductive polymer / PSS aqueous solution is 0.8% to 2.5%, and the mass percentage of PSS is 2.5% to 4.2%.

[0016] Further, in step S1, the M source is weighed according to the stoichiometric ratio, the molar ratio of the M element in the M source to the sodium element in the sodium source is 1:(1-1.05), and the chemical formula of the mixture 1 is Na x MO2, wherein 0.67≤X≤1, the M comprises at least one of Ni, Fe, Mn, Cu, and Co, the calcination atmosphere comprises air, the calcination temperature is 850°C to 950°C, and the calcination time is 10h to 20h.

[0017] Furthermore, in step S2, the mass ratio of the sodium element in the mixture 1 to the high molecular conductive polymer is 1:(0.01-0.09); the mass ratio of the water in the water washing kettle to the mixture 1 is (0.5-1.5):1.

[0018] Further, in step S2, the water in the water washing kettle includes deionized water;

[0019] And / or, in step S2, the stirring speed is 100-200 r / min, and the stirring time is 0.5h-1.5h;

[0020] And / or, in step S2, the mixture 1 is added to the water washing kettle after being crushed and screened, and the particle size range of the mixture 1 after crushing and screening is 9 μm to 13 μm.

[0021] Furthermore, in step S3, the drying temperature is 70-100° C., and the drying time is 3-5 hours.

[0022] In a second aspect, the present invention provides a modified sodium ion battery positive electrode material, characterized in that the modified sodium ion battery positive electrode material is prepared by the preparation method described in the first aspect, and the modified sodium ion battery positive electrode material comprises a sodium ion battery layered oxide positive electrode material and a coating, wherein the chemical formula of the sodium ion battery layered oxide positive electrode material is Na x MO2, 0.67≤X≤1, the M includes at least one of Ni, Fe, Mn, Cu, and Co, and the coating includes the high molecular conductive polymer.

[0023] In a third aspect, the present invention provides a sodium ion battery, characterized in that the positive electrode of the sodium ion battery comprises the modified sodium ion battery positive electrode material prepared by the preparation method described in the first aspect or the modified sodium ion battery positive electrode material described in the second aspect.

[0024] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:

[0025] (1) The present invention uses a water washing coating method to coat the layered oxide positive electrode material with a high molecular conductive polymer, thereby improving the gram capacity and cycle performance of the layered oxide positive electrode material.

[0026] (2) Compared with the prior art, the modified sodium ion battery positive electrode material provided by the present invention has a gram capacity of 135.1 mAh / g at 0.1C in the voltage range of 2.0-4.3V at room temperature of 25°C, and a capacity retention rate of 76% after 50 cycles at a current density of 0.1C / 0.5C, while the unmodified sodium ion battery positive electrode material has a gram capacity of 128.4 mAh / g at 0.1C under the same conditions, and a capacity retention rate of only about 68%, and its attenuation trend is greater than that of the modified sodium ion battery positive electrode material. The modified sodium ion battery positive electrode material has a higher gram capacity, better cycle performance, and less capacity attenuation.

[0027] (3) Compared with the prior art, the preparation method of the modified sodium ion battery positive electrode material provided by the present invention is relatively simple. The coating material used is a high molecular conductive polymer, which does not require secondary calcination after mixing with the positive electrode material, thereby reducing the production cost. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0029] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0030] In a first aspect, the present invention provides a method for preparing a modified sodium ion battery positive electrode material, the preparation method comprising the following steps:

[0031] S1, weighing an M source and a sodium source, mixing the M source and the sodium source evenly and then calcining to obtain a mixture 1 (layered oxide positive electrode material), wherein the M source includes at least one of a Ni source, a Fe source, a Mn source, a Cu source, and a Co source;

[0032] S2, adding a high molecular conductive polymer to the water in a water washing kettle, and then adding the mixture 1 to the water washing kettle, and obtaining a mixture 2 after stirring;

[0033] S3, centrifuging and drying the mixture 2 in step S2 to obtain a modified sodium ion battery positive electrode material.

[0034] The present invention coats the layered oxide positive electrode material with a high molecular conductive polymer by adopting a water washing coating method, thereby improving the gram capacity and cycle performance of the layered oxide positive electrode material.

[0035] The present invention uses a high molecular conductive polymer to perform surface coating modification on the layered oxide positive electrode material, which can form a short chain coating on the material surface. This short chain molecular chain is attached to the surface of the primary particle, which can effectively prevent moisture in the air from contacting the material surface, forming a barrier between the material surface and the outside world, inhibiting the exchange of sodium ions in the material bulk phase and protons in H2O, so that the bulk phase crystal structure remains stable, and the material cycle performance is improved. At the same time, the protective film formed by the high molecular conductive polymer on the material surface can inhibit the side reaction between the electrolyte and the material, and improve the material's gram capacity. The good conductivity of the high molecular conductive polymer will also make the sodium ion transmission rate faster, the sodium ion loss is less, and the material's gram capacity and initial efficiency are improved.

[0036] The preparation method provided by the present invention uses water as a solvent, directly adds a high molecular conductive polymer into pure water, and directly washes and coats the layered oxide positive electrode material, which can be well adapted to the existing ternary material production line. In addition, the residual alkali content on the surface of the positive electrode material after washing and coating is well controlled, the homogenized slurry has good stability, and the gas production in the later battery cell cycle is also reduced.

[0037] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional embodiment, the Ni source includes at least one of nickel sulfate and nickel nitrate, the Fe source includes at least one of iron sulfate and iron nitrate, the Mn source includes at least one of manganese sulfate and manganese nitrate, the Cu source includes at least one of copper sulfate and copper nitrate, the Co source includes at least one of cobalt sulfate and cobalt nitrate, and the sodium source includes at least one of sodium carbonate, sodium chloride, and sodium sulfate.

[0038] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional implementation, the high molecular conductive polymer includes at least one of PEDOT, polythiophene, and polypyrrole.

[0039] Specifically, PEDOT is a polymer of EDOT (3,4-ethylenedioxythiophene monomer), and the structural formula is as follows:

[0040]

[0041] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional implementation, in step S2, the high molecular conductive polymer is added to the water in the water washing kettle in the form of a high molecular conductive polymer / PSS (sodium polystyrene sulfonate) aqueous solution.

[0042] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional embodiment, in step S2, the mass percentage of the polymer conductive polymer in the aqueous solution of the polymer conductive polymer / PSS is 0.8% to 2.5%, preferably 1.5%, and the mass percentage of PSS is 2.5% to 4.2%, preferably 3.75%. PSS increases the solubility of PEDOT in water, so that PEDOT can form a uniformly dispersed aqueous solution with the mixture 1. If the PSS content is too high, the conductivity of the polymer conductive polymer / PSS will deteriorate.

[0043] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional embodiment, in step S1, the M source is weighed according to the stoichiometric ratio, the molar ratio of the M element in the M source to the sodium element in the sodium source is 1: (1 to 1.05), and the chemical formula of the mixture 1 is Na x MO2, wherein 0.67≤X≤1, the M comprises at least one of Ni, Fe, Mn, Cu, and Co, the calcination atmosphere comprises air, the calcination temperature is 850°C to 950°C (for example, 850°C, 870°C, 900°C, 920°C, or 950°C), and the calcination time is 10h to 20h (for example, 10h, 12h, 14h, 16h, 18h, or 20h).

[0044] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional embodiment, in step S2, the mass ratio of the sodium element in the mixture 1 (sodium ion battery layered oxide positive electrode material) to the high molecular conductive polymer is 1: (0.01-0.09), for example, it can be 1: 0.01, 1: 0.03, 1: 0.05, 1: 0.07 or 1: 0.09, preferably 1: (0.04-0.07); the mass ratio of the water in the water washing kettle to the mixture 1 is (0.5-1.5): 1, for example, it can be 0.5: 1, 0.8: 1, 1: 1, 1.3: 1 or 1.5: 1. If the amount of the high molecular conductive polymer is too much, it may cause the coating film to be thicker, which is not conducive to ion migration; too little content will lead to uneven coating or incomplete coating, affecting the coating effect. Too much water in the washing kettle will reduce the content of high molecular conductive polymer, affecting the coating effect. Too little water will make it impossible for the high molecular conductive polymer to be evenly dispersed and coated on the surface of the positive electrode material particles.

[0045] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional implementation, in step S2, the water in the water washing kettle includes deionized water.

[0046] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional implementation mode, in step S2, the stirring speed is 100 to 200 r / min (for example, it can be 100 r / min, 120 r / min, 140 r / min, 160 r / min, 180 r / min or 200 r / min), and the stirring time is 0.5 h to 1.5 h.

[0047] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional implementation, in step S2, the mixture 1 is added to the water washing kettle after crushing and screening, and the particle size range of the mixture 1 after crushing and screening is 9μm to 13μm. If the particle size of the mixture 1 is too small, more interface barriers need to be crossed during the sodium ion deintercalation process, which is not conducive to the performance of the gram capacity; if the particle size is too large, the structure is more likely to collapse during the deintercalation process, which is not conducive to the later cycle.

[0048] In the above-mentioned method for preparing the modified sodium ion battery positive electrode material, as an optional implementation, in step S3, the drying temperature is 70 to 100°C (for example, it can be 70°C, 80°C, 90°C or 100°C), and the drying time is 3 to 5 hours.

[0049] In a second aspect, the present invention provides a modified sodium ion battery positive electrode material, wherein the modified sodium ion battery positive electrode material is prepared by the preparation method described in the first aspect, and the modified sodium ion battery positive electrode material comprises a sodium ion battery layered oxide positive electrode material and a coating, wherein the chemical formula of the sodium ion battery layered oxide positive electrode material is Na x MO2, 0.67≤X≤1, the M includes at least one of Ni, Fe, Mn, Cu, and Co, and the coating includes a high molecular conductive polymer.

[0050] In the above-mentioned modified sodium ion battery positive electrode material, as an optional embodiment, the mass ratio of the sodium element in the sodium ion battery layered oxide positive electrode material to the high molecular conductive polymer is 1: (0.01-0.09), for example, it can be 1: 0.01, 1: 0.03, 1: 0.05, 1: 0.07 or 1: 0.09; the high molecular conductive polymer includes at least one of PEDOT, polythiophene, and polypyrrole.

[0051] In a third aspect, the present invention provides a sodium ion battery, wherein the positive electrode of the sodium ion battery comprises the modified sodium ion battery positive electrode material prepared by the preparation method described in the first aspect or the modified sodium ion battery positive electrode material described in the second aspect.

[0052] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0053] In the following examples and comparative examples:

[0054] The preparation method of the PEDOT / PSS aqueous solution includes the following steps: dissolving and dispersing PEDOT in PSS to obtain a PEDOT-PSS solution, and then adding the PEDOT-PSS solution into deionized water to obtain a PEDOT / PSS aqueous solution, wherein the mass percentage of PEDOT in the PEDOT / PSS aqueous solution is 1.5%, and the mass percentage of PSS is 3.75%.

[0055] Example 1

[0056] This embodiment provides a method for preparing a modified sodium ion battery positive electrode material, comprising the following steps:

[0057] S1. Nickel sulfate, iron sulfate, manganese sulfate and sodium sulfate were weighed according to the molar ratio of Ni:Fe:Mn:Na of 0.6:0.25:0.15:1.03, and nickel sulfate, iron sulfate, manganese sulfate and sodium sulfate were evenly mixed in the solid phase using an ultra-high-speed mixer. The obtained mixture was calcined at 910°C for 16 hours in an air atmosphere, and then pulverized by a jet mill after cooling, and sieved to obtain the layered oxide positive electrode material NaNi for sodium ion batteries. 0.6 Fe 0.25 Mn 0.15 O2 (mixture 1), wherein the particle size of the sodium ion battery layered oxide positive electrode material ranges from 9 μm to 13 μm;

[0058] S2, adding deionized water to the water washing kettle at a mass ratio of 0.8:1 to the sodium ion battery layered oxide positive electrode material, then adding the PEDOT / PSS aqueous solution to the deionized water in the water washing kettle, and then adding the sodium ion battery layered oxide positive electrode material obtained in step S1 to the water washing kettle, and obtaining a mixture 2 after stirring, wherein the mass ratio of the sodium element in the sodium ion battery layered oxide positive electrode material to the PEDOT is 1:0.04, the stirring speed is 150r / min, and the stirring time is 1h;

[0059] S3, conveying the mixture 2 in step S2 to a centrifuge for centrifugal dehydration, conveying the dehydrated mixture to a double cone vacuum dryer for rotary drying at 80° C. for 4 hours to obtain a modified sodium ion battery positive electrode material.

[0060] Example 2

[0061] The preparation method of the modified sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that, in step S2, the mass ratio of the sodium element in the sodium ion battery layered oxide positive electrode material to the PEDOT is 1:0.03.

[0062] Example 3

[0063] The preparation method of the modified sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that, in step S2, the mass ratio of the sodium element in the sodium ion battery layered oxide positive electrode material to the PEDOT is 1:0.05.

[0064] Example 4

[0065] The preparation method of the modified sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that, in step S2, the mass ratio of the sodium element in the sodium ion battery layered oxide positive electrode material to the PEDOT is 1:0.07.

[0066] Comparative Example 1

[0067] This comparative example provides a method for preparing a modified sodium ion battery positive electrode material, comprising the following steps:

[0068] Nickel sulfate, iron sulfate, manganese sulfate and sodium sulfate were weighed according to the molar ratio of Ni:Fe:Mn:Na of 0.6:0.25:0.15:1.03, and nickel sulfate, iron sulfate, manganese sulfate and sodium sulfate were evenly mixed in the solid phase using an ultra-high-speed mixer. The resulting mixture was calcined at 910°C for 16 hours in an air atmosphere, and then pulverized by a jet mill after cooling, and sieved to obtain the layered oxide positive electrode material NaNi for sodium ion batteries. 0.6 Fe 0.25 Mn 0.15 O2, wherein the particle size range of the sodium ion battery layered oxide positive electrode material is 9 μm to 13 μm.

[0069] Comparative Example 2

[0070] The preparation method of the modified sodium ion battery positive electrode material provided in this comparative example is basically the same as that in Example 1, except that, in step S2, the sodium ion battery layered oxide positive electrode material and the PEDOT powder are evenly mixed according to the mass ratio of the sodium element in the sodium ion battery layered oxide positive electrode material to the PEDOT of 1:0.04, stirred at 150r / min for 60min, and then rotary dried at 80°C in a double-cone vacuum dryer for 4h to obtain a modified sodium ion battery positive electrode material.

[0071] Comparative Example 3

[0072] The preparation method of the modified sodium ion battery positive electrode material provided in this comparative example is basically the same as that in Example 1, except that, in step S2, deionized water is added to the water washing kettle at a mass ratio of deionized water to sodium ion battery layered oxide positive electrode material of 3:1.

[0073] Performance Testing

[0074] The sodium ion battery positive electrode materials prepared in each embodiment and comparative example were prepared into button batteries, and their initial discharge capacity and cycle performance were tested. The specific test method is:

[0075] Preparation of positive electrode sheet: Sodium ion battery positive electrode material, SuperP and PVDF are mixed in a mass ratio of 90:5:5, and an appropriate amount of NMP is added and stirred evenly. The electrode slurry is evenly coated on aluminum foil, and then rolled and sliced ​​after drying, and vacuum dried at 120°C for 24 hours;

[0076] Button battery assembly: first place the positive electrode shell, place the shrapnel inside the shell, place the metal sheet on the shrapnel, place the φ12μm positive electrode sheet made above on the metal sheet, with the side coated with the positive electrode material facing up, infiltrated with electrolyte, covered with a φ16μm diaphragm (battery-grade polypropylene microporous film), then infiltrated with electrolyte, and place the metal lithium sheet; assemble into a CR2032 button battery; the electrolyte used is 1.15mol / LNaPF6 EC+DEC+EMC (volume ratio 1:1:1), and the additive DFP is 2%;

[0077] First discharge capacity test method: Under 25℃ environment, charge the assembled button cell at a constant current density of 0.1C to 4.3V, and then discharge it at a constant current density of 0.1C to 2.0V, and record the first discharge capacity and first coulomb efficiency.

[0078] Cycle performance test: At 25°C, charge the assembled button cell at a constant current density of 0.1C to 4.3V, and then discharge at a constant current density of 0.5C to 2.0V. Cycle 50 times and record the capacity retention rate. Capacity retention rate = gram capacity of discharge at the 50th cycle / gram capacity of discharge at the 1st cycle * 100%.

[0079] The test results are shown in Table 1.

[0080] Table 1

[0081]

[0082]

[0083] From Table 1 we can at least see that:

[0084] (1) By comparing Examples 1-4 with Comparative Example 1, it can be seen that the present invention improves the gram capacity and cycle performance of the layered oxide positive electrode material by coating the layered oxide positive electrode material with a high molecular conductive polymer using a water washing coating method. xThe cycle performance of MO2 has been greatly improved, which is mainly due to the fact that the coated polymer reduces the contact between sodium ions in the layered oxide and moisture in the air, inhibits the exchange of sodium ions and protons, ensures the stability of the layered structure of the material, and ultimately improves the cycle performance of the material; at the same time, the coated Na x The surface coating of MO2 material inhibits the side reactions between the electrolyte and the material surface, reduces the loss of sodium ions, and also improves the gram capacity and initial efficiency of the material to a certain extent.

[0085] (2) By comparing Example 1 with Comparative Example 2, it can be seen that the present invention can significantly improve the gram capacity and cycle performance of the layered oxide positive electrode material by adopting the water washing and coating method. The reason may be that the residual alkali content on the surface of the positive electrode material after water washing and coating provided by the method provided by the present invention is better controlled, the homogenized slurry has better stability, and the gas generation in the later battery cell cycle is also reduced.

[0086] (3) By comparing Example 1 with Comparative Example 3, it can be seen that when there is too much water in the water washing kettle, the gram capacity and cycle performance of the modified sodium ion battery obtained are reduced. The applicant speculates that the reason may be that too much water in the water washing kettle causes the PEDOT content to decrease, affecting the coating effect.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a modified sodium ion battery positive electrode material, characterized in that: The preparation method comprises the following steps: S1, weighing an M source and a sodium source, mixing the M source and the sodium source uniformly and then calcining to obtain a mixture 1, wherein the M source includes at least one of a Ni source, a Fe source, a Mn source, a Cu source, and a Co source; S2, adding a high molecular conductive polymer to the water in a water washing kettle, and then adding the mixture 1 to the water washing kettle, and obtaining a mixture 2 after stirring; S3, centrifuging and drying the mixture 2 in step S2 to obtain a modified sodium ion battery positive electrode material.

2. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: The Ni source includes at least one of nickel sulfate and nickel nitrate, the Fe source includes at least one of iron sulfate and iron nitrate, the Mn source includes at least one of manganese sulfate and manganese nitrate, the Cu source includes at least one of copper sulfate and copper nitrate, the Co source includes at least one of cobalt sulfate and cobalt nitrate, and the sodium source includes at least one of sodium carbonate, sodium chloride and sodium sulfate.

3. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: The high molecular conductive polymer includes at least one of PEDOT, polythiophene, and polypyrrole; And / or, in step S2, the high molecular conductive polymer is added to the water in the water washing kettle in the form of a high molecular conductive polymer / PSS aqueous solution.

4. The method for preparing the modified sodium ion battery positive electrode material according to claim 3, characterized in that: In step S2, the mass percentage of the high molecular conductive polymer in the high molecular conductive polymer / PSS aqueous solution is 0.8% to 2.5%, and the mass percentage of PSS is 2.5% to 4.2%.

5. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: In step S1, an M source is weighed according to a stoichiometric ratio, wherein the molar ratio of the M element in the M source to the sodium element in the sodium source is 1:(1-1.05), and the chemical formula of the mixture 1 is Na x MO2, wherein 0.67≤X≤1, the M comprises at least one of Ni, Fe, Mn, Cu, and Co, the calcination atmosphere comprises air, the calcination temperature is 850°C to 950°C, and the calcination time is 10h to 20h.

6. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: In step S2, the mass ratio of the sodium element in the mixture 1 to the high molecular conductive polymer is 1:(0.01-0.09); the mass ratio of the water in the water washing kettle to the mixture 1 is (0.5-1.5):

1.

7. The method for preparing a modified sodium ion battery positive electrode material according to claim 1, characterized in that: In step S2, the water in the water washing kettle includes deionized water; And / or, in step S2, the stirring speed is 100-200 r / min, and the stirring time is 0.5h-1.5h; And / or, in step S2, the mixture 1 is added to the water washing kettle after being crushed and screened, and the particle size range of the mixture 1 after crushing and screening is 9 μm to 13 μm.

8. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: In step S3, the drying temperature is 70-100° C., and the drying time is 3-5 hours.

9. A modified sodium ion battery positive electrode material, characterized in that: The modified sodium ion battery positive electrode material is prepared by the preparation method according to any one of claims 1 to 8, and the modified sodium ion battery positive electrode material comprises a sodium ion battery layered oxide positive electrode material and a coating, wherein the chemical formula of the sodium ion battery layered oxide positive electrode material is Na x MO2, 0.67≤X≤1, the M includes at least one of Ni, Fe, Mn, Cu, and Co, and the coating includes the high molecular conductive polymer.

10. A sodium ion battery, characterized in that: The positive electrode of the sodium ion battery comprises a modified sodium ion battery positive electrode material prepared by the preparation method described in any one of claims 1 to 8 or a modified sodium ion battery positive electrode material described in claim 9.

Citation Information

Patent Citations

  • Preparation method of sodium ion battery anode material

    CN103682320A

  • Polypyrrole-coated porous sodium manganate composite material, preparation method and application thereof

    CN110504437A

  • Sodium-ion battery nickel-based precursor capable of being used for filling conductive material and positive electrode material

    CN113871582A

  • Sodium ion positive electrode material and preparation method and application thereof

    CN114400309A

  • Composite positive electrode material for sodium ion battery and preparation method of composite positive electrode material

    CN115360344A