Carbon material and preparation method thereof, negative electrode current collector and application
By forming a porous structure on the surface layer of carbon material particles, doping metal ions and setting polar functional groups, the problem of insufficient alkaline metal capacity of conventional carbon materials is solved, and the Coulomb efficiency and energy density of alkali metal batteries are significantly improved.
Patent Information
- Application Number
- CN202410976828.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-19
AI Technical Summary
During the charging and discharging process of existing alkali metal batteries, due to the low alkaline metal capacity of conventional carbon materials, the alkali metal ions have a high nucleation barrier on their surface, which is not conducive to uniform deposition/peeling, resulting in low Coulomb efficiency and capacity maintenance. Low rate and low energy density.
By forming a porous structure on the surface of carbon material particles and doping metal ions into the porous structure layer, and at the same time, polar functional groups such as carbonyl, hydroxyl, nitro, phosphate, sulfonic acid and chlorine are provided on the surface to enhance the base Coulomb efficiency, capacity retention rate and mass energy density of metal batteries.
It effectively reduces the nucleation energy barrier of alkali metals on the surface of carbon materials, accelerates the solvation process, and improves the Coulomb efficiency, capacity retention rate and mass energy density of alkali metal batteries.
Smart Images

Figure CN118943378A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a carbon material and a preparation method thereof, a negative electrode current collector and applications thereof. Background Art
[0002] As the market demand for longer battery discharge time increases, the development of high energy density alkali metal battery technology has attracted much attention. However, alkali metal batteries face some technical difficulties in practical applications. During the charging and discharging process, the negative electrode side of the alkali metal battery needs to provide sufficient reaction sites and accommodation space for alkali metal deposition / stripping. Therefore, conductive carbon materials are usually used to construct a porous coating on the surface of the metal foil current collector on the negative electrode side. Conventional carbon materials have low affinity for alkali metals, resulting in a high nucleation barrier for alkali metal ions on their surface, which is not conducive to the uniform deposition / stripping of alkali metals on the surface of conventional carbon materials. Therefore, existing alkali metal batteries have problems such as low coulombic efficiency, low capacity retention rate and low energy density, which hinder their practical application.
[0003] Invention
[0004] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the purpose of the present application is to propose a carbon material and a preparation method thereof, a negative electrode current collector and application. The present application forms a porous structure on the surface of carbon material particles, dopes metal ions in the porous structure layer, and sets polar functional groups on the surface of the porous structure layer, thereby effectively improving the coulombic efficiency, capacity retention rate and mass energy density of alkali metal batteries.
[0005] In one aspect of the present application, the present application proposes a carbon material. According to an embodiment of the present application, the carbon material includes:
[0006] Carbon material particles, wherein the surface layer of the carbon material particles is a porous structure layer;
[0007] Metal ions, the metal ions are doped in the porous structure layer;
[0008] A polar functional group, wherein the polar functional group is distributed on the surface of the porous structure layer, and the polar functional group includes at least one of a carbonyl group, a hydroxyl group, a nitro group, a phosphoric acid group, a sulfonic acid group and a chlorine group.
[0009] According to the carbon material of the embodiment of the present application, a porous structure is formed on the surface of the carbon material particles, which increases the surface roughness and specific surface area of the carbon material, provides a large number of nucleation and deposition / stripping sites for alkali metals in the negative electrode current collector during the charge and discharge process, and is also conducive to the presence of metal ions in the form of doped elements on the surface of the carbon material particles. And doping metal ions in the porous structure layer can effectively reduce the nucleation energy barrier of alkali metals on the surface of the carbon material and accelerate the desolvation process of solvated alkali metal ion groups. At the same time, polar functional groups are set on the surface of the porous structure layer, which can further enhance the carbon material's affinity for alkali metals while also enhancing the carbon material's affinity for polar solvents and its dispersibility in the slurry. Overall, the modified carbon material of the present application can effectively improve the coulombic efficiency, capacity retention rate and mass energy density of alkali metal batteries.
[0010] In addition, the carbon material according to the above embodiment of the present application may also have the following additional technical features:
[0011] In some embodiments of the present application, the specific surface area of the carbon material particles is 1 m 2 / g-500m 2 / g.
[0012] In some embodiments of the present application, the pore size of the pores in the porous structure layer is 0-50 nm and is not equal to 0.
[0013] In some embodiments of the present application, the metal ions include at least one of iron ions, zinc ions, barium ions, tin ions and copper ions.
[0014] In some embodiments of the present application, based on the total mass of the carbon material being 100%, the mass proportion of the metal ions is 0.1%-5%.
[0015] In some embodiments of the present application, the carbon material particles include at least one of carbon nanotube particles, graphene particles, carbon fiber particles, conductive graphite particles, and carbon black particles.
[0016] In a second aspect of the present application, the present application proposes a method for preparing the above-mentioned carbon material. According to an embodiment of the present application, the method comprises:
[0017] preparing a modifier, the modifier comprising an oxidizing agent, a water-soluble metal salt and water;
[0018] The raw carbon material particles are mixed with the modifier, subjected to a modification treatment, and then the remaining modifier is removed to obtain the carbon material.
[0019] According to the method for preparing the above-mentioned carbon material in the embodiment of the present application, the original carbon material particles are modified by a modifier, so as to form a porous structure on the surface of the carbon material particles, increase the surface roughness and specific surface area of the carbon material, provide a large number of nucleation and deposition / stripping sites for alkali metals in the negative electrode current collector during the charge and discharge process, and also facilitate the metal ions to exist in the surface of the carbon material particles in the form of doped elements. And doping metal ions in the porous structure layer can effectively reduce the nucleation energy barrier of alkali metals on the surface of the carbon material and accelerate the desolvation process of the solvated alkali metal ion group. At the same time, polar functional groups are formed on the surface of the porous structure layer, which can further enhance the carbon material's affinity for alkali metals, and can also enhance the carbon material's affinity for polar solvents and its dispersibility in the slurry. Overall, the method for modifying carbon materials in the present application can effectively improve the coulombic efficiency, capacity retention rate and mass energy density of alkali metal batteries.
[0020] In addition, the method for preparing the above-mentioned carbon material according to the above-mentioned embodiment of the present application may also have the following additional technical features:
[0021] In some embodiments of the present application, the oxidizing agent includes at least one of phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, and acetic acid; and / or the water-soluble metal salt includes at least one of ferric nitrate, ferric sulfate, zinc nitrate, zinc sulfate, barium nitrate, barium chloride, tin nitrate, tin chloride, copper nitrate, and copper sulfate.
[0022] In some embodiments of the present application, the mass proportion of the oxidizing agent in the modifier is 20%-50%; and / or the mass proportion of the water-soluble metal salt in the modifier is 1%-10%.
[0023] In some embodiments of the present application, the temperature for the modification treatment is 20°C-120°C.
[0024] In the third aspect of the present application, the present application proposes a negative electrode current collector. According to an embodiment of the present application, the above-mentioned negative electrode current collector includes a current collector body; a functional layer, the functional layer is arranged on at least one side of the current collector body, and the functional layer includes the carbon material described in the above embodiment or includes the carbon material prepared by the method described in the above embodiment. Therefore, when the modified carbon material of the present application is used for the negative electrode current collector, the alkali metal nucleation overpotential during charging is significantly lower than that of the unmodified carbon material, and at the same time, the coulombic efficiency, capacity retention rate and mass energy density of the alkali metal battery can be effectively improved.
[0025] In addition, the negative electrode current collector according to the above embodiment of the present application may also have the following additional technical features:
[0026] In some embodiments of the present application, based on the total mass of the functional layer being 100%, the mass of the carbon material accounts for 70%-90%.
[0027] In the fourth aspect of the present application, the present application proposes an alkali metal battery. According to an embodiment of the present application, the above-mentioned alkali metal battery includes the negative electrode current collector described in the above embodiment. Thus, the coulombic efficiency, capacity retention rate and mass energy density of the alkali metal battery can be effectively improved.
[0028] In the fifth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device has the alkali metal battery described in the above embodiment. Therefore, the electrical device has all the advantages of the battery, which will not be repeated here.
[0029] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0031] Figure 1 A schematic diagram of the process of preparing carbon materials in some embodiments of the present application;
[0032] Figure 2 Schematic diagram of the structure of the negative electrode current collector of some embodiments of the present application.
[0033] Reference numerals:
[0034] 100-current collector body, 200-functional layer. DETAILED DESCRIPTION
[0035] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.
[0036] This application is proposed by the inventor based on the following issues:
[0037] Compared with metals such as zinc, barium, and iron, conventional carbon materials have lower affinity for alkali metals, resulting in a higher nucleation barrier for alkali metal ions on their surfaces, which is not conducive to the uniform deposition / stripping of alkali metals on the surfaces of conventional carbon materials. Therefore, the method of introducing metal particles with affinity for alkali metals into carbon materials can be used to improve the affinity for alkali metals of carbon materials. However, even nanoscale metal particles are composed of tens of thousands of metal atoms, and only a small number of atoms on the surface can play the role of affinity for alkali metals. The actual utilization rate is far less than 1%, and the overall mass energy density of the battery is also reduced due to its high density.
[0038] In view of this, in one aspect of the present application, the present application proposes a carbon material. According to an embodiment of the present application, the carbon material includes: carbon material particles, the surface layer of the carbon material particles is a porous structure layer; metal ions, the metal ions are doped in the porous structure layer; polar functional groups, the polar functional groups are distributed on the surface of the porous structure layer, and the polar functional groups include at least one of carbonyl, hydroxyl, nitro, phosphoric acid, sulfonic acid and chlorine. Therefore, the present application increases the surface roughness and specific surface area of the carbon material by forming a porous structure on the surface of the carbon material particles, providing a large number of nucleation and deposition / stripping sites for alkali metals in the negative electrode current collector during the charge and discharge process, and is also conducive to the presence of metal ions in the form of doped elements on the surface of the carbon material particles. And doping metal ions in the porous structure layer can effectively reduce the nucleation energy barrier of alkali metals on the surface of the carbon material and accelerate the desolvation process of the solvated alkali metal ion group. At the same time, polar functional groups are arranged on the surface of the porous structure layer, which can further improve the affinity of the carbon material for alkali metals, and can also improve the affinity of the carbon material for polar solvents and the dispersibility in the slurry. Overall, the modified carbon material of the present application can effectively improve the coulombic efficiency, capacity retention rate and mass energy density of alkali metal batteries.
[0039] The following is a detailed explanation of the principle by which the carbon material proposed in this application can achieve the above beneficial effects:
[0040] The preparation process of conventional carbon materials usually includes a high-temperature heat treatment step, so the surface of conventional carbon materials is usually dense and composed of non-polar carbon-carbon covalent bonds. The present application proposes a new type of modified carbon material, which includes carbon material particles, the surface layer of which is a porous structure layer. The porous structure in the porous structure layer increases the surface roughness and specific surface area of the carbon material, providing a large number of nucleation and deposition / stripping sites for alkali metals in the negative electrode current collector during charging and discharging.
[0041] At the same time, the surface layer of the carbon material particles is a porous structure layer, which is equivalent to the presence of a large number of structural defects in the surface layer of the carbon material particles, which is conducive to the penetration of metal ions in the porous structure layer using these defects as a breakthrough, and is conducive to the presence of metal ions in the form of doped elements (without forming nano or micron-sized particles) on the surface layer of the carbon material particles, thereby forming a carbon material doped with metal ions on the surface layer. There is a strong affinity between metal ions and alkali metal ions, so it is possible to reduce the nucleation energy barrier of alkali metals on the surface of carbon materials and accelerate the desolvation process of solvated alkali metal ion groups. When the modified carbon material of the present application is used as the negative electrode current collector of an alkali metal battery, the alkali metal nucleation overpotential during charging is significantly lower than that of the unmodified carbon material. In addition, there are no defects or metal ion doping inside the carbon material, so the electronic conductivity of the carbon material is not significantly reduced.
[0042] As mentioned above, metal ions exist in the form of doped elements on the surface of carbon material particles, and it is difficult for them to exist in the modified carbon material in the form of particles such as oxides and hydroxide precipitates. Therefore, the compaction density of the modified carbon material of the present application is lower than the compaction density of conventional carbon material + metal particle mixture / composite, and the weight of the prepared negative electrode current collector is lighter, thereby effectively improving the overall mass energy density of the alkali metal battery.
[0043] In addition, the surface of the porous structure layer (i.e., the surface of the carbon material) has a large number of polar functional groups, which can further enhance the carbon material's affinity for alkali metals while also enhancing the carbon material's affinity for polar solvents (such as deionized water) and its dispersibility in the slurry, thereby improving the coating slurry processing performance.
[0044] In an embodiment of the present application, the above-mentioned polar functional groups include at least one of carbonyl, hydroxyl, nitro, phosphate, sulfonate and chloride groups. While further enhancing the affinity of the carbon material to alkali metals, the polar functional groups can also enhance the affinity of the carbon material to polar solvents (such as deionized water) and its dispersibility in the slurry, thereby improving the processing performance of the coating slurry.
[0045] Therefore, compared with conventional carbon materials, the modified carbon materials of the present application have more surface defects, providing a large number of nucleation and deposition / stripping sites for alkali metals; the doped metal ions and polar functional groups on the surface of the modified carbon materials can effectively reduce the nucleation overpotential of alkali metals on the surface of the carbon materials. Overall, the modified carbon materials of the present application can effectively improve the coulombic efficiency, capacity retention rate and mass energy density of alkali metal batteries.
[0046] It should be noted that the surface of the porous structure layer refers to all surfaces of the carbon material particles, including the porous surfaces in the porous structure layer.
[0047] In the embodiments of the present application, the surface layer of the carbon material particles is a porous structure layer, and the porous structure in the porous structure layer increases the specific surface area of the carbon material particles. According to some specific embodiments of the present application, the specific surface area of the carbon material particles is 1m 2 / g-500m 2 / g, thereby further ensuring that a large number of nucleation and deposition / stripping sites are provided for alkali metals in the negative electrode current collector during the charge and discharge process, and further facilitating the penetration of metal ions into the surface layer of the porous structure.
[0048] In the embodiments of the present application, the porous structure of the surface layer of the above-mentioned carbon material particles is formed by attacking the dense surface of the carbon material with a modifier, so the pore sizes of the porous structure are different. As some specific embodiments, the pores in the porous structure layer have a pore size in the range of 0-50nm, and the pore size is not equal to 0.
[0049] In the embodiments of the present application, the types of the above-mentioned metal ions are not particularly limited, as long as they are water-soluble metal ions and have a strong affinity with alkali metal ions. As some preferred schemes, the metal ions include at least one of iron ions, zinc ions, barium ions, tin ions and copper ions. There is a strong affinity between the above-mentioned types of metal ions and alkali metal ions, so that the nucleation barrier of alkali metals on the surface of carbon materials can be further reduced, thereby accelerating the desolvation process of solvated alkali metal ion clusters.
[0050] According to some further specific embodiments of the present application, based on the total mass of the carbon material being 100%, the mass proportion of the metal ions is 0.1%-5%, for example, it can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc., thereby ensuring that a sufficient amount of metal elements are doped in the surface layer of the carbon material particles, thereby further ensuring that the nucleation energy barrier of the alkali metal on the surface of the carbon material is reduced, thereby accelerating the desolvation process of the solvated alkali metal ion clusters.
[0051] In the embodiments of the present application, the types of the above-mentioned carbon material particles are not particularly limited, and those skilled in the art can select them according to actual needs. As some preferred schemes, the carbon material particles include at least one of carbon nanotube particles, graphene particles, carbon fiber particles, conductive graphite particles, and carbon black particles.
[0052] In the second aspect of the present application, the present application proposes a method for preparing the above-mentioned carbon material. According to the embodiments of the present application, referring to the attached Figure 1 , the method comprising:
[0053] S100: Preparation of Modifier
[0054] In this step, a modifier is prepared, and the modifier includes an oxidizing agent, a water-soluble metal salt and water. Among them, the oxidizing agent itself has a strong oxidizing ability, and will attack the dense surface of the original carbon material particles during the modification process, thereby creating a large number of defects on the surface of the carbon material particles, forming a porous structure layer, thereby increasing the surface roughness and specific surface area of the carbon material, and providing a large number of nucleation and deposition / stripping sites for alkali metals. In addition, after being treated with the above-mentioned oxidizing agent, a large number of polar functional groups, such as carbonyl, hydroxyl, nitro, phosphoric acid, sulfonic acid, chlorine, etc., are formed on the surface of the modified carbon material, while further improving the carbon material's affinity for alkali metals, it also improves the carbon material's affinity for polar solvents and its dispersibility in the slurry, and improves the coating slurry processing performance.
[0055] The above-mentioned water-soluble metal salt is dissolved in water and ionized to form a large number of metal ions. After the oxidizing agent creates a large number of defects on the surface of the carbon material, the metal ions released by the water-soluble metal salt use these defects as a breakthrough point to penetrate into the surface of the carbon material, forming a carbon material doped with metal ions on the surface. There is a strong affinity between the metal ions and the alkali metal ions, so it can reduce the nucleation energy barrier of the alkali metal on the surface of the carbon material and accelerate the desolvation process of the solvated alkali metal ion group. In addition, there are no defects and metal ion doping inside the carbon material, and the electronic conductivity is not significantly reduced.
[0056] In the embodiments of the present application, the specific types of the above-mentioned oxidizing agents are not particularly limited. As some preferred schemes, the oxidizing agents include at least one of phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, and acetic acid. The above-mentioned oxidizing agents themselves have strong oxidizing ability. During the modification process, they will attack the dense surface of the original carbon material particles, thereby creating a large number of defects on the surface of the carbon material particles and forming a porous structure layer.
[0057] In the embodiments of the present application, the specific types of the above-mentioned water-soluble metal salts are not particularly limited. As some preferred schemes, the water-soluble metal salts include at least one of ferric nitrate, ferric sulfate, zinc nitrate, zinc sulfate, barium nitrate, barium chloride, tin nitrate, tin chloride, copper nitrate, and copper sulfate.
[0058] According to some specific embodiments of the present application, the mass proportion of the oxidizing agent in the modifier is 20%-50%, for example, it can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc. By limiting the mass proportion of the oxidizing agent in the modifier to the above range, it can further ensure that the oxidizing agent attacks the dense surface of the original carbon material particles during the modification process, thereby creating a large number of defects in the surface layer of the carbon material particles to form a porous structure layer.
[0059] According to some further specific embodiments of the present application, the mass proportion of the water-soluble metal salt in the modifier is 1%-10%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc. By limiting the mass proportion of the water-soluble metal salt in the modifier to the above range, it is possible to ensure that a sufficient amount of metal elements are doped in the surface layer of the carbon material particles, thereby further ensuring that the nucleation energy barrier of the alkali metal on the surface of the carbon material is reduced, thereby accelerating the desolvation process of the solvated alkali metal ion groups.
[0060] S200: Mix the original carbon material particles with the modifier and perform modification treatment
[0061] In this step, the original carbon material particles are mixed with a modifier and subjected to a modification treatment. The oxidizing agent will attack the dense surface of the original carbon material particles during the modification process, thereby creating a large number of defects on the surface of the carbon material particles to form a porous structure layer. After being treated with the above-mentioned oxidizing agent, a large number of polar functional groups will be formed on the surface of the modified carbon material. The metal ions released by the water-soluble metal salt use these defects as a breakthrough point to penetrate into the surface of the carbon material to form a carbon material doped with metal ions on the surface. The remaining modifier is then removed to obtain the carbon material.
[0062] According to some other specific embodiments of the present application, the temperature for the modification treatment is 20°C-120°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, etc. Within the above temperature range, the surface layer of the carbon material particles can be effectively modified.
[0063] In the embodiments of the present application, the time for the modification treatment depends on the temperature at which the modification treatment is performed and is not particularly limited, as long as it can ensure that the modification treatment of the carbon material particles is completed.
[0064] In the embodiments of the present application, the mass ratio of the original carbon material particles to the modifier is not particularly limited, as long as the original carbon material particles and the modifier are in full contact with each other, for example, the original carbon material particles can be immersed in the modifier.
[0065] According to the method for preparing the above-mentioned carbon material in the embodiment of the present application, the original carbon material particles are modified by a modifier, so as to form a porous structure on the surface of the carbon material particles, increase the surface roughness and specific surface area of the carbon material, provide a large number of nucleation and deposition / stripping sites for alkali metals in the negative electrode current collector during the charge and discharge process, and also facilitate the metal ions to exist in the surface of the carbon material particles in the form of doped elements. And doping metal ions in the porous structure layer can effectively reduce the nucleation energy barrier of alkali metals on the surface of the carbon material and accelerate the desolvation process of the solvated alkali metal ion group. At the same time, polar functional groups are formed on the surface of the porous structure layer, which can further enhance the carbon material's affinity for alkali metals, and can also enhance the carbon material's affinity for polar solvents and its dispersibility in the slurry. Overall, the method for modifying carbon materials in the present application can effectively improve the coulombic efficiency, capacity retention rate and mass energy density of alkali metal batteries.
[0066] In the third aspect of the present application, the present application provides a negative electrode current collector. According to the embodiments of the present application, referring to the attached Figure 2 , the above-mentioned negative electrode current collector includes a current collector body 200; a functional layer 100, the functional layer 100 is arranged on at least one side of the current collector body 200, and the functional layer 100 includes the carbon material described in the above embodiment or includes the carbon material prepared by the above method in the above embodiment. Therefore, when the modified carbon material of the present application is used for the negative electrode current collector, the alkali metal nucleation overpotential during charging is significantly lower than that of the unmodified carbon material, and at the same time, the coulombic efficiency, capacity retention rate and mass energy density of the alkali metal battery can be effectively improved.
[0067] According to some other specific embodiments of the present application, based on the total mass of the functional layer being 100%, the mass proportion of the carbon material is 70%-90%, for example, it can be 70%, 75%, 80%, 85%, 90%, etc. By limiting the mass proportion of the carbon material to the above range, it can be further ensured that the carbon material provides an efficient electron transmission path for the lithium / sodium deposition or stripping process, and at the same time provides a large number of nucleation and deposition / stripping sites for the alkali metal in the negative electrode current collector during the charge and discharge process.
[0068] Furthermore, the functional layer also includes a binder, which can effectively improve the bonding force between the functional layer and the substrate (ie, the current collector body) to prevent the functional layer from falling off.
[0069] In the embodiments of the present application, the specific types of the above-mentioned binders are not particularly limited, and those skilled in the art can select them according to actual needs. As some preferred schemes, the binders include at least one of polyvinylidene fluoride, polyacrylonitrile, polyimide, sodium carboxymethyl cellulose, styrene-butadiene rubber, sodium polyacrylate, sodium alginate, polytetrafluoroethylene, and polyvinyl alcohol.
[0070] According to some other specific embodiments of the present application, the thickness of the functional layer is 1 μm-50 μm, for example, it can be 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.
[0071] In the fourth aspect of the present application, the present application proposes an alkali metal battery. According to an embodiment of the present application, the above-mentioned alkali metal battery includes the negative electrode current collector described in the above embodiment. Thus, the coulombic efficiency, capacity retention rate and mass energy density of the alkali metal battery can be effectively improved.
[0072] In an embodiment of the present application, the alkali metal battery may be a lithium / sodium metal battery, which includes the negative electrode current collector described in the above embodiment, and the functional layer includes a modified carbon material. Thus, the coulombic efficiency, capacity retention rate and mass energy density of the lithium / sodium metal battery can be effectively improved.
[0073] The lithium / sodium metal battery can be a lithium metal battery or a sodium metal battery.
[0074] In the embodiments of the present application, the alkali metal battery may also be a negative electrode-free battery, which includes the negative electrode current collector described in the above embodiments, thereby effectively improving the coulombic efficiency, capacity retention rate and mass energy density of the negative electrode-free battery.
[0075] The above-mentioned negative electrode-free battery can be a negative electrode-free sodium ion battery or a negative electrode-free lithium ion battery. The following takes a negative electrode-free sodium ion battery as an example to illustrate that a negative electrode-free sodium ion battery refers to: de-sodiumizing the positive electrode material and depositing it in situ on the negative electrode current collector (in this application, it is deposited on the functional layer on the surface of the current collector body). No negative electrode active material is added during the production process, and only the negative electrode current collector is used as the nominal negative electrode. However, this negative electrode current collector does not have the function of a negative electrode. Only after the first charge is completed, the metal in the positive electrode material migrates to the surface of the negative electrode current collector (in this application, it migrates to the functional layer on the surface of the current collector body). The metal layer formed on the negative electrode current collector is the true negative electrode.
[0076] Specifically, the negative electrode-free battery includes a positive electrode sheet, a separator, a negative electrode current collector and an electrolyte, and the separator is arranged between the positive electrode sheet and the negative electrode current collector. The specific material of the separator is not particularly limited. As some specific examples, the separator includes at least one of a PP separator, a PE separator, a single-sided ceramic separator, a double-sided ceramic separator, a non-woven separator, and a glass fiber separator.
[0077] The positive electrode sheet includes a positive electrode current collector and a positive electrode material layer formed on the positive electrode current collector, wherein the positive electrode material layer includes a positive electrode active material, a positive electrode binder and a positive electrode conductor.
[0078] For sodium ion batteries, the positive electrode active material may include, but is not limited to, one or more of transition metal oxides, polyanionic compounds, organic polymers, and Prussian blue materials. In the sodium transition metal oxide, the transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. The sodium transition metal oxide is, for example, Na x MO2, where M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, 0<x≤1, for example, Na[Ni 1 / 3 Fe 1 / 3Mn 1 / 3 ]O2.
[0079] The polyanionic compound has sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds of anion units, the transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si; n represents (YO4) n- valence state, for example Na3V2(PO4)3.
[0080] The above-mentioned Prussian blue compounds are sodium ions, transition metal ions and cyanide ions (CN - ) is a class of compounds whose general chemical formula can be expressed as Na x M1[M2(CN)6], wherein 0<x≤2, M1 and M2 are at least one of Ni, Cu, Fe, Mn, Co and Zn respectively.
[0081] The specific material of the positive electrode binder is not particularly limited. As some specific examples, the positive electrode binder may include but is not limited to one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylonitrile (PAN), and polyacrylic acid (PAA).
[0082] The specific material of the positive electrode conductive agent is not particularly limited. As some specific examples, the positive electrode conductive agent may include but is not limited to one or more of acetylene black, conductive carbon black, carbon nanotubes, carbon fibers, graphene, and the like.
[0083] In the embodiments of the present application, the specific material of the positive electrode current collector is not particularly limited. As some specific examples, the positive electrode current collector may include but is not limited to at least one of aluminum foil, carbon-coated aluminum foil, and stainless steel foil.
[0084] In the embodiments of the present application, the electrolyte includes electrolyte salt and organic solvent, wherein the specific types and compositions of the electrolyte salt and organic solvent are conventional choices in the battery field and can be selected according to actual needs.
[0085] In some embodiments, the electrolyte salt may include, but is not limited to, at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium bis(trifluoromethanesulfonyl)imide (NaN(CF3SO2)2), sodium bis(fluorosulfonyl)imide (NaN(SO2F)2), sodium bis(oxalatoborate) (NaB(C2O4)2), and sodium difluorooxalatoborate (NaBF2C2O4).
[0086] In some embodiments, the organic solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), diethylene glycol dimethyl ether (DEGDME), ethylene glycol dimethyl ether (DME), 1,3-dioxolane (DOL), and tetraethylene glycol dimethyl ether (TEGDME).
[0087] The battery of the present application may include a battery cell form, a battery module form and a battery pack form. In some embodiments, the battery cells can be assembled into a battery module, and the number of battery cells contained in the battery module can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module. In some embodiments, the battery modules can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0088] In the fifth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device has the alkali metal battery described in the above embodiment. Therefore, the electrical device has all the advantages of the battery, which will not be repeated here.
[0089] Specifically, the electrical equipment may be, but is not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, etc. Electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft may include airplanes, rockets, space shuttles, and spacecraft, etc.
[0090] The embodiments of the present application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. In addition, unless otherwise explicitly stated, all reagents used in the following embodiments are commercially available or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0091] Example 1
[0092] This embodiment provides a battery, and the preparation method thereof includes:
[0093] 1. Preparation of modified carbon materials
[0094] An oxidizing agent (nitric acid), a water-soluble metal salt (ferric nitrate) and deionized water are mixed in a certain mass ratio to form a modifier, carbon material particles and the modifier are mixed in a mass ratio of 20:100, heated at 80 degrees Celsius for 24 hours, and then the modifier is removed to obtain a modified carbon material.
[0095] 2. Preparation of negative electrode current collector
[0096] The modified carbon material, the conductive agent (Ketjen black) and the polyvinylidene fluoride are mixed in a mass ratio of 80:10:10, and N-methylpyrrolidone solvent is added and stirred into a uniform slurry with a solid content of 10%. The slurry is coated on an aluminum foil using a coater and dried in an oven. The current collector is cold pressed by a roller press to obtain a functional coating with a thickness of 20 μm.
[0097] 3. Preparation of positive electrode sheet
[0098] The active material (sodium vanadium phosphate), conductive agent (ketjen black), and binder (PVDF) are mixed evenly in a stirring device at a mass ratio of 90:3:7, and then a certain amount of solvent (nitrogen methyl pyrrolidone) is added and stirred to form a uniform slurry with a solid content of 40%. The slurry is coated on the positive electrode current collector aluminum foil using a coating machine, dried, and cold pressed to obtain a positive electrode sheet.
[0099] 4. Prepare electrolyte
[0100] In an argon-protected glove box, take 1 L of diethylene glycol dimethyl ether into a volumetric flask; weigh 168 g of sodium hexafluorophosphate and dissolve it in the above solvent; stir thoroughly until the sodium salt is completely dissolved to obtain the desired electrolyte.
[0101] 5. Diaphragm
[0102] A 16 μm polyethylene film was used as the separator.
[0103] 6. Assemble half-cell
[0104] Use a circular hole slicer to punch out the positive electrode sheet, negative electrode current collector, and separator into small discs of different diameters; put the negative electrode current collector, separator, and metal sodium sheet into the button battery shell in order, with the separator between the negative electrode current collector and the metal sodium sheet, add the above-mentioned electrolyte, and assemble into a button half-cell.
[0105] 7. Assemble the full battery
[0106] The positive electrode sheet, separator, and negative electrode current collector are stacked in order, with the separator located between the positive electrode sheet and the negative electrode current collector, and the above-mentioned electrolyte is added to assemble a full battery.
[0107] Example 2-Example 23
[0108] The preparation methods of the modified carbon materials and batteries of Examples 2 to 23 are the same as those of Example 1, and the differences are detailed in Table 1.
[0109] Comparative Examples 1-3
[0110] The preparation methods of the carbon materials and batteries in Comparative Examples 1-3 are the same as those in Example 1, and the differences are detailed in Table 1.
[0111] The carbon material in Comparative Example 1 was not modified.
[0112] In the modifier of Comparative Example 2, no water-soluble metal salt is added.
[0113] No oxidizing agent is added to the modifier of Comparative Example 3.
[0114] The parameters of the carbon materials of Examples 1-23 and Comparative Examples 1-3 are listed in Table 1.
[0115] Table 1
[0116]
[0117] The performance of Examples 1-23 and Comparative Examples 1-3 were tested respectively, and the test results are shown in Table 2. The test process is as follows:
[0118] 1. Specific surface area of carbon materials
[0119] The specific surface area and pore size distribution of the material are determined by nitrogen low temperature adsorption method. The sample is placed in the specific surface area tester for testing and the isothermal adsorption and desorption curve is obtained to calculate the specific surface area, pore structure and other information of the sample.
[0120] 2. Mass proportion of metal ions in carbon materials
[0121] The metal ion content in the material is determined by inductively coupled plasma atomic emission spectrometry. After the sample is digested, it is introduced into the plasma emission spectrometer, and its intensity is measured at the corresponding element wavelength. The metal element content in the sample is calculated using the standard curve method, and the metal element mass fraction is converted.
[0122] 3. Types of polar groups on the surface of carbon material particles
[0123] Fourier transform infrared spectroscopy is used to determine the types of polar groups on the surface of the material. After the powder sample is pressed into a tablet, it is tested in an infrared spectrometer, and the types of polar groups in the sample are calibrated according to the positions of the characteristic peaks of the infrared spectrum.
[0124] 4. Test method for nucleation overpotential
[0125] The half-cell was tested with constant current charge and discharge on a battery charge and discharge tester, with the charge and discharge current set to 1 mA / cm 2 , the discharge cut-off capacity is set to 2 mAh / cm 2 , the charging cut-off voltage is set to 1.5V.
[0126] 5. Test method for 100-cycle average coulomb efficiency
[0127] The whole battery is subjected to constant current charge and discharge test on the battery charge and discharge tester; the ratio of the discharge capacity of the nth cycle of the battery / the charging capacity of the nth cycle is the nth cycle coulomb efficiency; the average value of the coulomb efficiency from the 1st cycle to the 100th cycle is the average coulomb efficiency.
[0128] 6. Test method for 100-cycle capacity retention rate
[0129] The full battery is subjected to constant current charge and discharge test on a battery charge and discharge tester; the ratio of the battery's 100th cycle discharge capacity / 1st cycle discharge capacity is the capacity retention rate.
[0130] Table 2
[0131]
[0132]
[0133] In addition, the pore sizes of the pores in the porous structure layer of the modified carbon materials of Examples 1-23 were tested by a nitrogen low temperature adsorption method and were found to be in the range of 0-50 nm and not equal to 0.
[0134] It can be seen from Table 1 and Table 2 that the carbon material in Comparative Example 1 is not treated with a modifier, the carbon material modifier in Comparative Example 2 does not contain a metal salt, and the carbon material modifier in Comparative Example 3 does not contain an oxidizing agent.
[0135] The carbon material modifiers in Examples 1 to 20 contain both an oxidizing agent and a metal salt. From the test results, it can be seen that the nucleation overpotentials of Examples 1 to 20 are all lower than those of Comparative Examples 1 to 3, and the average coulombic efficiency and capacity retention rate are all higher than those of Comparative Examples 1 to 3, indicating that the present application uses a method of modifying carbon materials using a combined modifying agent to improve the lithium / sodium affinity of the negative electrode current collector, reduce the nucleation overpotential, and induce uniform deposition of metal lithium / sodium.
[0136] It can be seen from Comparative Example 3 and Examples 1-4 that the present application can reduce the nucleation overpotential and improve the average coulombic efficiency and capacity retention rate of the battery by adjusting the proportion of the oxidizing agent in the modifier. The mass proportion of the oxidizing agent in the modifier is limited to 30%-50%, which has a stronger ability to reduce the nucleation overpotential and induce uniform deposition of metallic lithium / sodium, and also has a stronger effect of improving the average coulombic efficiency and capacity retention rate of the battery.
[0137] It can be seen from Examples 3 and 5-8 that the present application can reduce the nucleation overpotential and improve the average coulombic efficiency and capacity retention rate of the battery by adjusting the proportion of the metal salt in the modifier. When the mass proportion of the metal salt in the modifier is in the range of 3%-10%, the ability to reduce the nucleation overpotential and induce uniform deposition of metal lithium / sodium is stronger, and the effect of improving the average coulombic efficiency and capacity retention rate of the battery is also stronger.
[0138] As can be seen from Example 3 and Example 9-12, the present application can reduce the nucleation overpotential and improve the average coulombic efficiency and capacity retention rate of the battery by adjusting the type of oxidizing agent in the modifier. Different types of oxidizing agents have different abilities to oxidize carbon materials and different etching abilities to the surface of carbon materials. Among them, nitric acid and sulfuric acid have strong oxidizing abilities, modified carbon materials have high specific surface areas, and the proportion of metal elements is also high, so the nucleation overpotential is low, and the average coulombic efficiency and capacity retention rate are high. In addition, the comparison between Example 3 and Example 10 shows that the type of sodium-philic groups on the surface of the carbon material also affects the nucleation overpotential. In Example 10, the type of sodium-philic groups on the surface of the modified carbon material is more, the nucleation overpotential is low, and the ability to induce uniform deposition of metal lithium / sodium is stronger, so its average coulombic efficiency and capacity retention rate are higher.
[0139] It can be seen from Example 3 and Examples 13-16 that the present application can reduce the nucleation overpotential and improve the average coulombic efficiency and capacity retention rate of the battery by adjusting the type of metal salt in the modifier. When the types of metal salts in the modifier are different, the types of metal elements on the surface of the modified carbon material are different, and their ability to alkali metals in the subsequent lithium / sodium deposition process is different. Metal elements with strong sodium affinity (such as Example 15) have a stronger ability to reduce the nucleation overpotential than metal elements with weak sodium affinity (such as Example 16), and the average coulombic efficiency and capacity retention rate are also higher.
[0140] It can be seen from Example 3 and Examples 17-20 that the present application can reduce the nucleation overpotential and improve the average coulombic efficiency and capacity retention rate of the battery by adjusting the modification temperature of the carbon material. The modification temperature in the range of 50°C-120°C can further reduce the nucleation overpotential and further improve the average coulombic efficiency and capacity retention rate of the battery.
[0141] It can be seen from Example 3 and Examples 21-23 that the present application can reduce the nucleation overpotential and improve the average coulombic efficiency and capacity retention rate of the battery by adjusting the type of initial carbon material.
[0142] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0143] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A carbon material, characterized in that include: Carbon material particles, wherein the surface layer of the carbon material particles is a porous structure layer; Metal ions, the metal ions are doped in the porous structure layer; A polar functional group, wherein the polar functional group is distributed on the surface of the porous structure layer, and the polar functional group includes at least one of a carbonyl group, a hydroxyl group, a nitro group, a phosphoric acid group, a sulfonic acid group and a chlorine group.
2. The carbon material according to claim 1, characterized in that The specific surface area of the carbon material particles is 1m 2 / g-500m 2 / g.
3. The carbon material according to claim 1, characterized in that The pore diameter of the pores in the porous structure layer is 0-50 nm and is not equal to 0.
4. The carbon material according to claim 1, characterized in that The metal ions include at least one of iron ions, zinc ions, barium ions, tin ions, and copper ions.
5. The carbon material according to claim 1, characterized in that Based on the total mass of the carbon material being 100%, the mass proportion of the metal ions is 0.1%-5%.
6. The carbon material according to any one of claims 1 to 5, characterized in that The carbon material particles include at least one of carbon nanotube particles, graphene particles, carbon fiber particles, conductive graphite particles, and carbon black particles.
7. A method for preparing the carbon material according to any one of claims 1 to 6, characterized in that: include: preparing a modifier, the modifier comprising an oxidizing agent, a water-soluble metal salt and water; The raw carbon material particles are mixed with the modifier, subjected to a modification treatment, and then the remaining modifier is removed to obtain the carbon material.
8. The method according to claim 7, characterized in that The oxidizing agent includes at least one of phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, and acetic acid; And / or, the water-soluble metal salt includes at least one of ferric nitrate, ferric sulfate, zinc nitrate, zinc sulfate, barium nitrate, barium chloride, tin nitrate, tin chloride, copper nitrate and copper sulfate.
9. The method according to claim 7, characterized in that: The mass proportion of the oxidizing agent in the modifier is 20%-50%; And / or, the mass proportion of the water-soluble metal salt in the modifier is 1%-10%.
10. The method according to any one of claims 7 to 9, characterized in that: The temperature for the modification treatment is 20°C-120°C.
11. A negative electrode current collector, characterized in that: include: Current collector body; A functional layer is provided on at least one side of the current collector body, and the functional layer comprises the carbon material according to any one of claims 1 to 6 or the carbon material prepared by the method according to any one of claims 7 to 10.
12. The negative electrode current collector according to claim 11, characterized in that: Based on the total mass of the functional layer being 100%, the mass of the carbon material accounts for 70%-90%.
13. An alkali metal battery, characterized in that: Comprising the negative electrode current collector according to claim 11 or 12.
14. An electrical device, characterized in that: An alkali metal battery according to claim 13.
Citation Information
Patent Citations
Applications of porous carbon material in lithium-thionyl chloride battery positive electrode
CN104518218A
Preparation method of graphite oxide phase carbon nitride modified electrode and application of electrode in detection of heavy metal ions
CN104634836A
Composite negative electrode material, preparation method thereof and lithium ion battery
CN117832463A
Cylinder type storage battery
JP2003168473A