Novel microcrystal composite alloy catalyst material and preparation method thereof

The mesoporous graphite microcrystalline carrier material was prepared through arc technology and electron cyclotron resonance technology, and the nano alloy was loaded, which solved the problem of insufficient activity and durability of existing fuel cell catalyst carrier materials, and achieved efficient and rapid catalyst production and electrochemical performance promote.

CN118943394APending Publication Date: 2024-11-12GUANGZHOU MOXI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310534775.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In actual applications, existing fuel cell catalyst support materials such as carbon black and graphene have problems such as insufficient catalyst activity, insufficient durability and increased battery internal resistance, and lack of suitable pore structures and good connection between the support and the catalyst, which limits the Catalyst properties.

Method used

Using arc technology and electron cyclonic resonance technology to prepare mesoporous graphite microcrystalline support materials, and grow alloy particles on it to form mesoporous graphite microcrystalline support particles, and load nano alloys to build suitable porous structures to improve the activity of the catalyst. and stability.

Benefits of technology

It realizes efficient and rapid production of catalyst materials, improves the activity and electrochemical durability of the catalyst, ensures the uniform distribution and stability of alloy particles, can withstand high static pressure, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943394A_ABST
    Figure CN118943394A_ABST
Patent Text Reader

Abstract

The invention relates to a novel microcrystal composite alloy catalyst and a preparation method thereof, the novel microcrystal composite alloy catalyst comprises a large amount of graphite microcrystals, nano-alloy on the graphite microcrystals and 2-50nm mesopores among the graphite microcrystals, the pore size D50 is 15nm, and the structure enables the catalyst to have a very high specific surface area and good nano-alloy dispersibility. The catalyst has excellent catalytic activity and excellent electrochemical corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a novel microcrystalline composite alloy catalyst material and a preparation method thereof. Background Art

[0002] Alloy catalysts are considered to be one of the most effective fuel cell catalysts at present. The simplification of their preparation process, reduction of costs, and improvement of activity and durability will greatly improve the availability of fuel cells in practical applications. Alloy catalysts are composed of catalytically active alloy particles and carbon carriers, of which the carbon carrier constitutes the skeleton of the entire catalyst layer and has an important influence on the activity and durability of the catalyst. The ideal catalyst carrier should have the following characteristics: 1. Good electrical conductivity; 2. Large specific surface area; 3. Reasonable pore structure; 4. Strong corrosion resistance; 5. Good connection and interaction between the carrier and the catalyst.

[0003] Among the common catalyst carrier materials currently available, carbon black has the advantages of good electrical conductivity, large specific surface area, and rich void structure. However, it still has its limitations in practical applications. For example, the incompatible pore size will lead to insufficient utilization of the loaded catalyst active particles, and the platinum atoms on its surface are prone to migration and agglomeration, which in turn leads to a decrease in catalyst activity. In addition, although activated carbon has good electrical conductivity, it also has limitations, which will lead to an increase in the internal resistance of the battery, and its application in fuel cell carriers will also be limited. Therefore, the selection of a good carrier will have an extremely important positive impact on the performance of the catalyst.

[0004] Graphene has good mechanical properties and electrical conductivity due to its special layered structure and the presence of freely movable π electrons, and has the characteristics of strong corrosion resistance and large specific surface area. However, ordinary graphene is a two-dimensional film and cannot be directly used as a catalyst. The present invention constructs a special two-dimensional nano and three-dimensional mesoporous structure through an original method to form a suitable porous microcrystalline material. This characteristic will enable it to simultaneously ensure sufficient active sites, stable nano alloy loading, and ultra-high electrochemical durability. In addition, it can contain controllable nitrogen and oxygen through doping, which can provide a large number of adsorption sites to anchor alloy particles, thereby loading alloy particles in a large amount and evenly dispersed manner, and further improve activity and electrochemical stability. Summary of the invention

[0005] The present invention aims to provide a novel microcrystalline composite alloy catalyst material and a preparation method thereof. Firstly, arc technology and electron cyclotron resonance technology are combined to rapidly and massively produce mesoporous microcrystalline carbon carrier materials, and then alloy particles are directly grown on the carrier materials.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions: A novel microcrystalline composite alloy catalyst material comprises graphite microcrystals, mesopores between graphite microcrystals, mesoporous graphite microcrystal carrier particles composed of graphite microcrystals and mesopores, and nano-alloys loaded on graphite microcrystals. The novel microcrystalline composite alloy catalyst material is composed of mesoporous graphite microcrystal carrier particles and the nano-alloys loaded therein.

[0007] The graphite microcrystals are petal-shaped, with a flake size of 10-30 nm and a thickness of 3-5 nm.

[0008] The mesopore size between the graphite microcrystals is 2-50 nm, and the pores with a mesopore size of <15 nm account for ≥50% of the total pore volume, the most probable (largest number) mesopore size is <3 nm, and the average pore diameter is ≤15 nm.

[0009] The specific surface area of ​​the mesoporous graphite microcrystal carrier particles composed of graphite microcrystals and mesopores is 200-500 m 2 / g, total pore volume is 2~3cm 3 / g.

[0010] The graphite microcrystals are doped with 1-3 wt.% of nitrogen, and the content of oxygen is less than 1 wt.%.

[0011] The particle size of the mesoporous graphite microcrystalline carrier particles and the catalyst material is 50-200 nm, preferably 100-150 nm.

[0012] The alloy catalyst includes any one of a platinum alloy catalyst and a single atom catalyst.

[0013] The platinum alloy catalyst includes any one of a platinum-palladium alloy, a platinum-cobalt alloy, and a platinum-nickel alloy.

[0014] The single-atom catalyst includes any one of iron phthalocyanine, cobalt phthalocyanine, and iron-cobalt phthalocyanine.

[0015] The size of the platinum-palladium alloy is 2-4 nm, the size of the platinum-cobalt alloy is 2-8 nm, the size of the platinum-nickel alloy is 2-4 nm, the size of the iron phthalocyanine particles is 2-4 nm, the size of the cobalt phthalocyanine particles is 2-4 nm, and the size of the iron-cobalt phthalocyanine particles is 2-4 nm. The alloy particles are evenly and fully distributed in the mesoporous graphite microcrystalline carrier particles.

[0016] The graphite microcrystals and mesopores completely maintain their original structures and sizes when forming mesoporous graphite microcrystal carrier particles and novel microcrystal composite alloy catalyst materials, wherein the graphite microcrystals do not form agglomeration and stacking, and the mesopores do not collapse or expand.

[0017] Furthermore, the mesoporous graphite microcrystal carrier particle structure composed of graphite microcrystals and mesopores can withstand a maximum static pressure of 100MPa, that is, applying a maximum static pressure of 100MPa to the material will not destroy the microstructure of the material. After releasing the pressure, the particle structure and size of the mesoporous graphite microcrystal carrier remain intact, while protecting the alloy particles therein as well, that is, the new microcrystalline composite alloy catalyst material can withstand a maximum static pressure of 100MPa.

[0018] In one embodiment, the process comprises the following steps: using arc-enhanced electron cyclotron resonance plasma as a reaction medium, using Ketjen black as a raw material, argon as a carrier gas, hydrogen as an etching gas, and oxygen and ammonia as doping gases, to first prepare a mesoporous graphite microcrystalline carrier particle material. Figure 3~4 Shown 1) Using argon as carrier gas, Ketjen black (model: ECP-600) powder is transported to the arc gun as a precursor (plasma gas 1). The argon gas is ionized in the arc gun to form an argon plasma arc. The high-temperature arc generated vaporizes and ionizes the Ketjen black in it to form a mixed arc of argon and carbon. The arc is directly sprayed into the electron cyclotron resonance plasma chamber as a precursor for subsequent processes. Figure 3 Shown 2) Hydrogen, oxygen and ammonia (plasma gas 2) enter the electron cyclotron resonance plasma chamber, form plasma under the dual cracking action of electron cyclotron resonance and the aforementioned arc, mix with the plasma entering the chamber in 1), and then reach a substrate to which a radio frequency bias is applied, and deposit on the substrate to form a mesoporous graphite microcrystal carrier particle material, wherein the carbon plasma forms graphite microcrystals, argon plasma is used to assist the gasification and ionization of Ketjen black, and to regulate the microstructure and size of the material, hydrogen plasma is used to regulate the size of the mesopores and graphite microcrystals, and oxygen plasma is used to dope oxygen elements on the graphite microcrystals.

[0019] 3) Taking the substrate out of the cavity and collecting the mesoporous graphite microcrystalline carrier particle material on the substrate.

[0020] In one embodiment, the content of all metal impurities in the mesoporous graphite microcrystalline support particle material is less than 20 ppm.

[0021] In one embodiment, alloy particles are synthesized and prepared directly in a mesoporous graphite microcrystalline carrier particle material using an in-situ growth method, and the alloy particles are uniformly loaded on the nanosheets, with a loading amount adjustable from 1 to 75%, to obtain a novel microcrystalline composite alloy catalyst.

[0022] Compared with the prior art, the present invention has the following beneficial effects: 1) The technical method of the present invention is efficient and fast, and can achieve rapid industrial mass production.

[0023] 2) The material of the present invention has: mesoporous structure, high specific surface area and high graphitization characteristics, which greatly improves the activity and stability of the catalyst material.

[0024] 3) The material of the present invention can control the content of nitrogen and oxygen doping, with the nitrogen content being 1-3% and the oxygen content being <1%, thereby significantly improving the activity and service life of the catalyst, and the oxygen content will not have a negative impact.

[0025] Figure 1 , Appearance photo of the novel microcrystalline composite alloy catalyst material of the present invention Figure 2 , Scanning electron microscope photo of the microstructure of the novel microcrystalline composite alloy catalyst material of the present invention Figure 3 Schematic diagram of the arc gun structure used in the present invention Figure 4 Schematic diagram of the electron cyclotron resonance cavity structure used in the present invention Figure 5 TEM photos of new mesoporous microcrystalline carbon composite platinum-palladium alloy catalyst material Figure 6 , LSV data comparison of new mesoporous microcrystalline carbon composite platinum-palladium alloy catalyst material Figure 7 , Data chart of 6000 cycles of new mesoporous microcrystalline carbon composite platinum-palladium alloy catalyst material Figure 8 , Anode oxygen release curve of water electrolysis using new mesoporous microcrystalline carbon composite platinum-cobalt alloy catalyst material Fig. 9 , LSV data comparison of new mesoporous microcrystalline carbon composite phthalocyanine iron cobalt catalyst material In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present invention, but are not intended to limit the present invention. Implementation

[0026] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Unless otherwise defined, technical or scientific terms used in the present disclosure shall have the common meanings understood by those having ordinary skills in the field to which the present invention belongs.

[0028] Example 1 Preparation of a novel mesoporous microcrystalline carbon composite platinum-palladium alloy metal catalyst material and its ORR performance test By Figure 3 and 4 The plasma gas 1 and 2 are firstly introduced into the gas inlet with a flow rate of 1 slm to remove the air in the cavity and fill the entire cavity with argon gas, and then the argon gas flow rate is closed. Figure 3 4.33slm of argon carrier gas was introduced into the plasma port 1 shown in the figure, in which 1g / min of Ketjen black (model: ECP-600) was mixed, the nozzle aperture of the arc gun was 1.2mm, the current of the arc power supply was set to a pulse current of 204A, the voltage was 73.5V, the single pulse time was 40μs, and the duty cycle was 50%. Figure 4 Hydrogen, oxygen and ammonia gases are introduced into the two ports of each plasma as shown in the figure. The flow rate of hydrogen is 7.79 slm, the flow rate of oxygen is 21 sccm, and the flow rate of ammonia is 21 sccm. The frequency of microwaves in the electron cyclotron resonance cavity is 2.45 GHz, and the initial mode of microwaves is TE 10 The rectangular mode is then converted using a microwave polarizer into a right-hand-rule TE at 2.45 GHz. 11 The circular waveguide mode is introduced by the dielectric windows around the cavity as indicated by the arrows in the figure. The power at each window is 1000W, the magnetic field strength of the multipolar magnetic field is 875G, the temperature in the resonance zone is 1600℃, the substrate is a graphite substrate, the RF bias on the substrate is 27MHz, 500W, and the gas pressure in the electron cyclotron resonance cavity is 1mtorr. The raw materials generate plasma in the arc gun and the electron cyclotron resonance cavity and are mixed in the cavity to achieve the reaction deposition of mesoporous graphite microcrystalline carrier particle material on the graphite substrate. After 30 minutes, 27g of mesoporous graphite microcrystalline carrier particle material is obtained, with a nitrogen content of 1.5~2% and an oxygen content of 0.5%. After being taken out, it is collected from the graphite substrate.

[0029] Preparation of a new mesoporous microcrystalline carbon composite platinum-palladium alloy catalyst material: 1) Take a 1L reaction container, dissolve 13gH2PtCl6▪6H2O and 5gPdCl2 in 450mL ethylene glycol, and stir evenly (stir for 1h); 2) Take a clean beaker, weigh 28gNaOH and dissolve it in 450mL ethylene glycol, stir evenly (stir for 1h), then add 10g of the mesoporous microcrystalline carbon carrier prepared in the above process, stir for 2h, and ultrasonicate for 1h; 3) Start preheating the oil bath to 160℃. 4) Add 2 to 1 and stir evenly (stir for 0.5h); 5) Close the container, connect the gas pipe, pass Ar / N2 gas, the gas flow rate is about 2L / min, and the condenser is cooled by water. 6) Put the entire reaction container into an oil bath preheated to 160℃, start stirring, so that the stirring speed keeps the liquid flowing without vortex, continue to ventilate, and react for 1.5h. 7) Turn off the heating, wait until the temperature drops below 80°C, turn off the gas, stir, and condense the water. 8) Take out the reaction product, add 900mL of dilute hydrochloric acid to mix, centrifuge at a speed of 10,000 rpm, take the precipitate and add 900mL of dilute hydrochloric acid to mix, centrifuge, then rinse with deionized water and dry to obtain a new mesoporous microcrystalline carbon composite nano-platinum-palladium alloy catalyst material with a platinum-palladium loading of 50%. Its TEM photo is as follows: Figure 5 shown.

[0030] The ORR performance of the catalyst material was tested using a rotating disk electrode. The test results are as follows Figure 6 As shown, it can be seen from the LSV curve that the material has excellent ORR performance, wherein curve 2 is the catalyst performance of Johnson Matthey with 60% platinum loading, and curve 1 is the performance of the new mesoporous microcrystalline carbon composite nano-platinum catalyst of this embodiment. Figure 7 The CV and LSV data after 6000 cycles at high potential show that the catalyst material of the present invention has excellent cycle performance and maintains more than 90% of its performance after 6000 cycles.

[0031] Example 2 Preparation of a novel mesoporous microcrystalline carbon composite platinum-cobalt alloy catalyst material and its performance in oxygen production By Figure 3 and 4 The plasma gas 1 and 2 are firstly introduced into the gas inlet with a flow rate of 1 slm to remove the air in the cavity and fill the entire cavity with argon gas, and then the argon gas flow rate is closed. Figure 3 4.33slm of argon carrier gas was introduced into the plasma port 1 shown in the figure, in which 1g / min of Ketjen black (model: ECP-600) was mixed, the nozzle aperture of the arc gun was 1.2mm, the current of the arc power supply was set to a pulse current of 204A, the voltage was 73.5V, the single pulse time was 40μs, and the duty cycle was 50%. Figure 4As shown in the figure, hydrogen, oxygen and ammonia are introduced into the two ports of each plasma. The flow rate of hydrogen is 7.79 slm, the flow rate of oxygen is 32 sccm, the flow rate of ammonia is 32 sccm, the frequency of microwaves in the electron cyclotron resonance cavity is 2.45 GHz, and the initial mode of microwaves is TE 10 The rectangular mode is then converted using a microwave polarizer into a right-hand-rule TE at 2.45 GHz. 11 The circular waveguide mode is introduced by the dielectric windows around the cavity as indicated by the arrows in the figure. The power at each window is 1000W, the magnetic field strength of the multipolar magnetic field is 875G, the temperature in the resonance zone is 1200℃, the substrate is a graphite substrate, the RF bias on the substrate is 27MHz, 500W, and the gas pressure in the electron cyclotron resonance cavity is 1mtorr. The raw materials generate plasma in the arc gun and the electron cyclotron resonance cavity and are mixed in the cavity to achieve the reaction deposition of mesoporous graphite microcrystalline carrier particle material on the graphite substrate. After 30 minutes, 27g of mesoporous graphite microcrystalline carrier particle material is obtained, with a nitrogen content of 2~3% and an oxygen content of <1%. After being taken out, it is collected from the graphite substrate.

[0032] Preparation of a new mesoporous microcrystalline carbon composite platinum-cobalt alloy catalyst material: 1) Take a 1L reaction container, dissolve 15g H2PtCl6▪6H2O and 6g CoCl2▪6H2O in 500mL ethylene glycol, and stir evenly (stir for 1h); 2) Take a clean beaker, weigh 10g PVP and dissolve it in 500mL ethylene glycol, stir evenly (stir for 1h), then add 1.5g of the mesoporous microcrystalline carbon carrier prepared in the above process, stir for 2h, and ultrasonicate for 1h; 3) Start preheating the oil bath to 120℃. 4) Add 2 to 1 and stir evenly (stir for 0.5h); 5) Close the container, connect the gas pipe, pass Ar / N2 gas, the gas flow rate is about 2L / min, and the condenser is cooled by water. 6) Put the entire reaction container into an oil bath preheated to 120℃, heat for 20min, then raise the temperature to 195℃, make the stirring speed keep the liquid flowing without vortex, continue to ventilate, and react for 1h. 7) Turn off the heating, wait until the temperature drops below 80°C, turn off the gas, stir, and condense the water. 8) Take out the reaction product, add 500 mL of acetone to mix, centrifuge at a speed of 10,000 rpm, take the precipitate and add 500 mL of acetone to mix and centrifuge, then rinse with deionized water and dry to obtain a new mesoporous microcrystalline carbon composite nano-platinum-cobalt alloy catalyst material with a platinum-cobalt loading of 50%.

[0033] The electrolytic water performance of the catalyst material was tested using a rotating disk electrode. The test results are as follows Figure 8As shown in the figure, it can be seen from the LSV curve that the material has excellent ORR performance, wherein curve 1 is the catalyst performance of the conductive carbon black carrier with 50% platinum-cobalt alloy loading, and curve 2 is the performance of the novel mesoporous microcrystalline carbon composite platinum-cobalt alloy catalyst of this embodiment. It can be seen that the catalyst of the present invention has a smaller oxygen evolution overpotential and better activity.

[0034] Example 3 Preparation of a novel mesoporous microcrystalline carbon composite platinum-nickel alloy catalyst material and its performance in hydrogen production By Figure 3 and 4 The plasma gas 1 and 2 are firstly introduced into the gas inlet with a flow rate of 1 slm to remove the air in the cavity and fill the entire cavity with argon gas, and then the argon gas flow rate is closed. Figure 3 4.33slm of argon carrier gas was introduced into the plasma port 1 shown in the figure, in which 1g / min of Ketjen black (model: ECP-600) was mixed, the nozzle aperture of the arc gun was 1.2mm, the current of the arc power supply was set to a pulse current of 204A, the voltage was 73.5V, the single pulse time was 40μs, and the duty cycle was 50%. Figure 4 Hydrogen and oxygen gases are introduced into the two ports of each plasma shown in the figure. The flow rate of hydrogen is 7.79 slm, the flow rate of oxygen is 1 sccm, the frequency of microwaves in the electron cyclotron resonance cavity is 2.45 GHz, and the initial mode of microwaves is TE 10 The rectangular mode is then converted using a microwave polarizer into a right-hand-rule TE at 2.45 GHz. 11 The circular waveguide mode is introduced by the dielectric windows around the cavity as indicated by the arrows in the figure. The power at each window is 1000W, the magnetic field strength of the multipolar magnetic field is 875G, the temperature in the resonance zone is 2800℃, the substrate is a graphite substrate, the RF bias on the substrate is 27MHz, 500W, and the gas pressure in the electron cyclotron resonance cavity is 1mtorr. The raw materials generate plasma in the arc gun and the electron cyclotron resonance cavity and are mixed in the cavity to achieve the reaction deposition of mesoporous graphite microcrystalline carrier particle material on the graphite substrate. After 30 minutes, 27g of mesoporous graphite microcrystalline carrier particle material is obtained, and its oxygen content is <0.1%, which is collected from the graphite substrate after being taken out.

[0035] Preparation of a new mesoporous microcrystalline carbon composite platinum-nickel alloy catalyst material: 1) Take a 1L reaction container, dissolve 14mmolH2PtCl6▪6H2O and 14mmolNiCl2▪6H2O in 500mL ethylene glycol, and stir evenly (stir for 1h); 2) Take a clean beaker, weigh 20g PVP and dissolve it in 500mL ethylene glycol, stir evenly (stir for 1h), then add 1.5g of the mesoporous microcrystalline carbon carrier prepared in the above process, stir for another 2h, and ultrasonicate for 1h; 3) Start preheating the oil bath to 160℃. 4) Put 2 in an oil bath preheated to 160℃, heat for 30min, then quickly inject 1 into 2, keep the stirring speed to keep the liquid flowing without vortex, continue to ventilate Ar, and react for 1h. 7) Turn off the heating and use an ice water bath to quickly cool down. 8) Take out the reaction product, add 500mL acetone to mix, centrifuge at 10,000 rpm, take out the precipitate, add 500mL acetone to mix, centrifuge, rinse with deionized water and dry, and obtain a new mesoporous microcrystalline carbon composite platinum-nickel alloy catalyst material with a platinum-nickel loading of 50%. Use a pulse reactor to test the conversion frequency (TOF) of the catalyst material to decompose methanol to produce hydrogen at room temperature, and the result can be as high as 200mol H2 mol -1 Pd min -1 . Example 4 Preparation of a novel mesoporous microcrystalline carbon composite iron phthalocyanine catalyst material and its performance in oxygen production By Figure 3 and 4 The plasma gas 1 and 2 are firstly introduced into the gas inlet with a flow rate of 1 slm to remove the air in the cavity and fill the entire cavity with argon gas, and then the argon gas flow rate is closed. Figure 3 4.33slm of argon carrier gas was introduced into the plasma port 1 shown in the figure, in which 1g / min of Ketjen black (model: ECP-600) was mixed, the nozzle aperture of the arc gun was 1.2mm, the current of the arc power supply was set to a pulse current of 204A, the voltage was 73.5V, the single pulse time was 40μs, and the duty cycle was 50%. Figure 4 Hydrogen and oxygen gases are introduced into the two ports of each plasma as shown in the figure. The flow rate of hydrogen is 7.79 slm, the flow rate of oxygen is 21 sccm, the frequency of microwaves in the electron cyclotron resonance cavity is 2.45 GHz, and the initial mode of microwaves is TE 10 The rectangular mode is then converted using a microwave polarizer into a right-hand-rule TE at 2.45 GHz. 11The circular waveguide mode is introduced by the dielectric windows around the cavity as indicated by the arrows in the figure. The power at each window is 1000W, the magnetic field strength of the multipolar magnetic field is 875G, the temperature in the resonance zone is 1600℃, the substrate is a graphite substrate, the RF bias on the substrate is 27MHz, 500W, and the gas pressure in the electron cyclotron resonance cavity is 1mtorr. The raw materials generate plasma in the arc gun and the electron cyclotron resonance cavity and are mixed in the cavity to achieve the reaction deposition of mesoporous graphite microcrystalline carrier particle material on the graphite substrate. After 30 minutes, 27g of mesoporous graphite microcrystalline carrier particle material is obtained, and its oxygen content is 2%. After being taken out, it is collected from the graphite substrate.

[0036] Preparation of a new mesoporous microcrystalline carbon composite phthalocyanine iron catalyst material: 1) Take a 1L reaction container, 6gC 32 H 16 1) Dissolve FeN8 in 300 mL DMF and stir evenly (stir for 1 hour). 2) Add 3 g of the mesoporous microcrystalline carbon carrier prepared in the above process, stir for another 1 hour, ultrasonicate for 1 hour, and continue stirring for 15 hours; 3) Obtain the reaction product by filtration, then rinse with ethanol several times, and dry the obtained sample in a vacuum at 60°C for 12 hours to obtain a new mesoporous microcrystalline carbon composite iron phthalocyanine catalyst material with an iron phthalocyanine loading of 50%.

[0037] Example 5 Preparation of a novel mesoporous microcrystalline carbon composite phthalocyanine iron cobalt catalyst material and its performance in oxygen production By Figure 3 and 4 The plasma gas 1 and 2 are firstly introduced into the gas inlet with a flow rate of 1 slm to remove the air in the cavity and fill the entire cavity with argon gas, and then the argon gas flow rate is closed. Figure 3 4.33slm of argon carrier gas was introduced into the plasma port 1 shown in the figure, in which 1g / min of Ketjen black (model: ECP-600) was mixed, the nozzle aperture of the arc gun was 1.2mm, the current of the arc power supply was set to a pulse current of 204A, the voltage was 73.5V, the single pulse time was 40μs, and the duty cycle was 50%. Figure 4 Hydrogen and oxygen gases are introduced into the two ports of each plasma as shown in the figure. The flow rate of hydrogen is 7.79 slm, the flow rate of oxygen is 21 sccm, the frequency of microwaves in the electron cyclotron resonance cavity is 2.45 GHz, and the initial mode of microwaves is TE 10 The rectangular mode is then converted using a microwave polarizer into a right-hand-rule TE at 2.45 GHz. 11The circular waveguide mode is introduced by the dielectric windows around the cavity as indicated by the arrows in the figure. The power at each window is 1000W, the magnetic field strength of the multipolar magnetic field is 875G, the temperature in the resonance zone is 1600℃, the substrate is a graphite substrate, the RF bias on the substrate is 27MHz, 500W, and the gas pressure in the electron cyclotron resonance cavity is 1mtorr. The raw materials generate plasma in the arc gun and the electron cyclotron resonance cavity and are mixed in the cavity to achieve the reaction deposition of mesoporous graphite microcrystalline carrier particle material on the graphite substrate. After 30 minutes, 27g of mesoporous graphite microcrystalline carrier particle material is obtained, and its oxygen content is 2%. After being taken out, it is collected from the graphite substrate.

[0038] Preparation of a new mesoporous microcrystalline carbon composite phthalocyanine iron cobalt catalyst material: 1) Take a 500 mL reaction container, 0.3 g C 32 H 16 FeN8 and 0.3gC 32 H 16 1) Dissolve CoN8 in 200 mL of DMF and stir evenly (stir for 1 hour); 2) Add 2.4 g of the mesoporous microcrystalline carbon carrier prepared in the previous process, stir for another 1 hour, ultrasonicate for 1 hour, and continue stirring for 15 hours; 3) Obtain the reaction product by filtration, then rinse with ethanol several times, and dry the obtained sample in a vacuum at 60°C for 12 hours to obtain a new mesoporous microcrystalline carbon composite phthalocyanine iron cobalt catalyst material with a phthalocyanine iron cobalt loading of 50%.

[0039] The ORR performance of the catalyst material was tested using a rotating disk electrode. The test results are as follows Fig. 9 As shown, it can be seen from the LSV curve that the material has excellent ORR performance, wherein the black curve is the catalyst performance of Johnson Matthey with 60% platinum loading, the blue curve is the catalyst performance of graphene, and the red curve is the catalyst performance of the new mesoporous microcrystalline carbon composite phthalocyanine iron cobalt of this embodiment.

Claims

1. A novel microcrystalline composite alloy catalyst, comprising graphite microcrystals, mesopores between graphite microcrystals, mesoporous graphite microcrystal carrier particles composed of graphite microcrystals and mesopores, and nano-alloys loaded on graphite microcrystals. The novel microcrystalline composite alloy catalyst is composed of mesoporous graphite microcrystal carrier particles and the nano-alloys loaded therein.

2. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The graphite microcrystals are nanometer-sized graphite microchips, the size of which is 10-30 nm, and the thickness of which is 3-5 nm.

3. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The mesopore size between the graphite microcrystals is 2-50 nm, and the pores with a mesopore size of <15 nm account for ≥50% of the total pore volume, the most probable (largest number) mesopore size is <3 nm, and the average pore diameter is ≤15 nm.

4. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The specific surface area of ​​the mesoporous graphite microcrystal carrier particles composed of graphite microcrystals and mesopores is 200~500m 2 / g, total pore volume is 2~3cm 3 / g.

5. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The graphite microcrystals are doped with 1-3 wt.% of nitrogen, and the content of oxygen is less than 1 wt.%.

6. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The particle size of the mesoporous graphite microcrystalline carrier particles and the catalyst material is 50-200 nm, preferably 100-150 nm.

7. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The alloy catalyst includes a platinum alloy catalyst, wherein the platinum alloy catalyst includes any one of a platinum-palladium alloy, a platinum-cobalt alloy, and a platinum-nickel alloy.

8. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The metal alloy catalyst includes a single-atom catalyst, wherein the single-atom catalyst includes any one of iron phthalocyanine, cobalt phthalocyanine, and iron-cobalt phthalocyanine.

9. The novel mesoporous microcrystalline carbon composite precious metal catalyst material according to claim 1, It is characterized in that The size of the platinum-palladium alloy is 2-4 nm, the size of the platinum-cobalt alloy is 2-8 nm, the size of the platinum-nickel alloy is 2-4 nm, the size of the iron phthalocyanine particles is 2-4 nm, the size of the cobalt phthalocyanine particles is 2-4 nm, and the size of the iron-cobalt phthalocyanine particles is 2-4 nm. The alloy particles are evenly and fully distributed in the mesoporous graphite microcrystalline carrier particles.

10. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The graphite microcrystals and mesopores completely maintain their original structures and sizes when forming mesoporous graphite microcrystal carrier particles and novel microcrystal composite alloy catalyst materials, wherein the graphite microcrystals do not form agglomeration and stacking, and the mesopores do not collapse or expand.

11. The novel microcrystalline composite alloy catalyst material according to claim 1, It is characterized in that The mesoporous graphite microcrystal carrier particle structure composed of graphite microcrystals and mesopores can withstand a maximum static pressure of 100MPa, that is, applying a maximum static pressure of 100MPa to the material will not destroy the material's microstructure. After the pressure is released, the structure and size of the mesoporous graphite microcrystal carrier particles remain intact, while the nano-alloys therein are also protected intact, that is, the new microcrystalline composite alloy catalyst material can withstand a maximum static pressure of 50MPa.

12. A novel microcrystalline composite alloy catalyst material according to claim 1, Features The production process includes the following steps: using arc-enhanced electron cyclotron resonance plasma as a reaction medium, using Ketjen black as a raw material, argon as a carrier gas, hydrogen as an etching gas, and oxygen as a doping gas, first preparing a mesoporous graphite microcrystalline carrier particle material. As shown in Figures 3 and 4 1) Using argon as carrier gas, Ketjen black (model: ECP-600) powder is transported to the arc gun as a precursor (plasma gas 1). Argon is ionized in the arc gun to form an argon plasma arc. The high-temperature arc generated vaporizes and ionizes the Ketjen black therein to form a mixed arc of argon and carbon. The arc is directly sprayed into the electron cyclotron resonance plasma chamber as a precursor for subsequent processes. As shown in Figure 3, 2) Hydrogen, oxygen, and ammonia (plasma gas 2) enter the electron cyclotron resonance plasma chamber, and form plasma under the dual cracking action of electron cyclotron resonance and the aforementioned arc, and mix with the plasma entering the chamber in 1), and then reach the substrate with an RF bias applied, and deposit on the substrate to form a mesoporous graphite microcrystalline carrier particle material, in which the carbon plasma forms graphite microcrystals, and the argon plasma is used to assist the gasification and ionization of Ketjen black, as well as to regulate the microstructure and size of the material, the hydrogen plasma is used to regulate the size of the mesopores and graphite microcrystals, and the oxygen plasma is used to dope the graphite microcrystals with oxygen elements. 3) Taking the substrate out of the cavity and collecting the mesoporous graphite microcrystalline carrier particle material on the substrate.

13. The novel microcrystalline composite alloy catalyst material according to claims 1 to 11, It is characterized in that The content of all metal impurities in the mesoporous graphite microcrystalline carrier particle material is less than 20 ppm.

14. The novel microcrystalline composite alloy catalyst material according to claims 1 to 11, It is characterized in that The alloy nanoparticles are synthesized and prepared directly in the mesoporous graphite microcrystalline carrier particle material using an in-situ growth method. The alloy nanoparticles are uniformly loaded on the nanosheets, and the loading amount is adjustable from 1 to 75%, thereby obtaining a new type of microcrystalline composite alloy catalyst.

Citation Information

Cited By

  • Novel mesoporous nano platinum-carbon catalyst

    CN117334936A